3920 | 3919 | 3918 | 3917 | 3911 | 3910 | 3908 | 3909 | 3907 | 3901 | 3902 | 3904 | 3899 | 3898 | 3897 | 3896 | 3895 | 3893 | 3890 | 3891 | 3892 | 3888 | 3889 | 3883 | 3885 | 3882 | 3880 | 3881 | 3878 | 3876 | 3871 | 3872 | 3874 | 3869 | 3870 | 3866 | 3867 | 3864 | 3863 | 3862 | 3861 | 3860 | 3859 | 3838 | 3857 | 3858 | 3855 | 3856 | 3851 | 3853 | 3854 | 3849 | 3850 | 3852 | 3846 | 3848 | 3843 | 3840 | 3841 | 3842 | 3837 | 3836 | 3833 | 3831 | 3832 | 3829 | 3827 | 3828 | 3826 | 3824 | 3823 | 3822 | 3820 | 3819 | 3818 | 3815 | 3816 | 3817 | 3814 | 3813 | 3811 | 3810 | 3806 | 3807 | 3808 | 3805 | 3803 | 3802 | 3801 | 3800 | 3797 | 3798 | 3796 | 3793 | 3794 | 3792 | 3789 | 3786 | 3784 | 3787 | 3781 | 3779 | 3775 | 3773 | 3774 | 3772 | 3767 | 3768 | 3769 | 3762 | 3760 | 3759 | 3755 | 3752 | 3753 | 3754 | 3750 | 3748 | 3749 | 3742 | 3743 | 3745 | 3746 | 3747 | 3740 | 3737 | 3738 | 3736 | 3734 | 3733 | 3732 | 3731 | 3729 | 3728 | 3726 | 3725 | 3724 | 3723 | 3721 | 3719 | 3720 | 3718 | 3716 | 3713 | 3712 | 3711 | 3710 | 3709 | 3707 | 3708 | 3706 | 3705 | 3704 | 3702 | 3701 | 3700 | 3699 | 3698 | 3695 | 3696 | 3697 | 3692 | 3693 | 3694 | 3690 | 3691 | 3689 | 3688 | 3685 | 3686 | 3679 | 3678 | 3676 | 3675 | 3674 | 3672 | 3673 | 3663 | 3664 | 3661 | 3656 | 3657 | 3658 | 3659 | 3651 | 3652 | 3654 | 3655 | 3650 | 3649 | 3648 | 3646 | 3647 | 3644 | 3645 | 3643 | 3642 | 3640 | 3639 | 3637 | 3636 | 3634 | 3635 | 3632 | 3631 | 3629 | 3630 | 3626 | 3627 | 3624 | 3625 | 3622 | 3623 | 3620 | 3619 | 3612 | 3610 | 3611 | 3606 | 3607 | 3608 | 3609 | 3602 | 3603 | 3604 | 3605 | 3601 | 3600 | 3599 | 3598 | 3596 | 3595 | 3594 | 3593 | 3591 | 3592 | 3588 | 3589 | 3585 | 3586 | 3584 | 3580 | 3581 | 3582 | 3583 | 3579 | 3577 | 3578 | 3576 | 3574 | 3572 | 3573 | 3571 | 3570 | 3568 | 3567 | 3565 | 3562 | 3563 | 3560 | 3561 | 3559 | 3557 | 3556 | 3555 | 3554 | 3553 | 3551 | 3552 | 3550 | 3549 | 3548 | 3547 | 3546 | 3544 | 3545 | 3543 | 3542 | 3538 | 3539 | 3540 | 3541 | 3536 | 3537 | 3535 | 3534 | 3531 | 3532 | 3533 | 3529 | 3530 | 3527 | 3528 | 3526 | 3525 | 3524 | 3523 | 3522 | 3520 | 3518 | 3516 | 3517 | 3515 | 3514 | 3512 | 3513 | 3511 | 3510 | 3509 | 3508 | 3507 | 3506 | 3505 | 3504 | 3046 | 3503 | 3493 | 3494 | 3490 | 3491 | 3486 | 3489 | 3485 | 3481 | 3483 | 3492 | 3479 | 3480 | 3476 | 3477 | 3474 | 3473 | 3471 | 3470 | 3469 | 3468 | 3465 | 3466 | 3467 | 3463 | 3459 | 3460 | 3461 | 3462 | 3458 | 3457 | 3456 | 3455 | 3454 | 3452 | 3449 | 3448 | 3447 | 3446 | 3445 | 3443 | 3444 | 3442 | 3441 | 3439 | 3440 | 3437 | 3438 | 3435 | 3436 | 3431 | 3433 | 3434 | 3430 | 3427 | 3428 | 3425 | 3426 | 3424 | 3423 | 3422 | 3419 | 3421 | 3418 | 3415 | 3416 | 3417 | 3414 | 3413 | 3411 | 3412 | 3409 | 3410 | 3408 | 3401 | 3402 | 3403 | 3404 | 3406 | 3407 | 3400 | 3399 | 3397 | 3393 | 3394 | 3396 | 3392 | 3391 | 3387 | 3389 | 3390 | 3385 | 3384 | 3383 | 3382 | 3379 | 3380 | 3381 | 3378 | 3376 | 3375 | 3374 | 3373 | 3372 | 3370 | 3367 | 3368 | 3369 | 3364 | 3363 | 3360 | 3359 | 3358 | 3356 | 3355 | 3354 | 3352 | 3349 | 3348 | 3347 | 3344 | 3345 | 3346 | 3343 | 3342 | 3340 | 3338 | 3339 | 3337 | 3335 | 3336 | | 3333 | 3330 | 3322 | 3319 | 3320 | 3321 | 3317 | 3316 | 3313 | 3314 | 3315 | 3312 | 3310 | 3311 | 3309 | 3307 | 3308 | 3306 | 3304 | 3303 | 3302 | 3300 | 3301 | 3298 | 3299 | 3296 | 3295 | 3293 | 3294 | 3292 | 3291 | 3290 | 3289 | 3288 | 3286 | 3285 | 3284 | 3280 | 3281 | 3282 | 3278 | 3277 | 3272 | 3273 | 3274 | 3275 | 3276 | 3271 | 3270 | 3267 | 3268 | 3265 | 3266 | 3264 | 3262 | 3261 | 3260 | 3259 | 3258 | 3257 | 3256 | 3255 | 3253 | 3254 | 3251 | 3248 | 3249 | 3247 | 3245 | 3246 | 3244 | 3241 | 3239 | 3236 | 3237 | 3235 | 3234 | 3233 | 3231 | 3232 | 3230 | 3229 | 3201 | 3202 | 3203 | 3204 | 3205 | 3206 | 3207 | 3208 | 3209 | 3210 | 3211 | 3212 | 3213 | 3214 | 3215 | 3216 | 3217 | 3219 | 3220 | 3222 | 3223 | 3224 | 3226 | 3227 | 3228 | 3199 | 3198 | 3197 | 3195 | 3196 | 3191 | 3192 | 3193 | 3194 | 3188 | 3189 | 3187 | 3185 | 3186 | 3183 | 3181 | 3182 | 3179 | 3180 | 3177 | 3176 | 3175 | 3174 | 3173 | 3169 | 3167 | 3164 | 3162 | 3159 | 3158 | 3157 | 3154 | 3155 | 3156 | 3153 | 3149 | 3150 | 3144 | 3145 | 3146 | 3147 | 3148 | 3142 | 3143 | 3139 | 3141 | 3138 | 3136 | 3137 | 3132 | 3135 | 3131 | 3130 | 3127 | 3124 | 3125 | 3126 | 3122 | 3123 | 3121 | 3120 | 3117 | 3119 | 3116 | 3112 | 3113 | 3114 | 3109 | 3110 | 3111 | 3098 | 3099 | 3102 | 3103 | 3104 | 3105 | 3106 | 3107 | 3108 | 3096 | 3094 | 3095 | 3091 | 3092 | 3093 | 3089 | 3090 | 3087 | 3086 | 3082 | 3083 | 3084 | 3080 | 3081 | 3079 | 3078 | 3077 | 3074 | 3075 | 3076 | 3073 | 3072 | 3070 | 3053 | 3055 | 3056 | 3057 | 3058 | 3059 | 3060 | 3061 | 3062 | 3063 | 3064 | 3065 | 3066 | 3067 | 3068 | 3069 | 3052 | 3050 | 3051 | 3048 | 3049 | 3047 | 3044 | 3043 | 3042 | 3041 | 3040 | 3038 | 3039 | 3037 | 3036 | 3035 | 3034 | 3033 | 3029 | 3030 | 3031 | 3023 | 3024 | 3021 | 3022 | 3019 | 3016 | 3017 | 3018 | 3015 | 3012 | 3013 | 3014 | 3011 | 3010 | 3007 | 3008 | 3009 | 3005 | 3006 | 3004 | 3001 | 3002 | 3003 | 2999 | 2995 | 2996 | 2994 | 2991 | 2992 | 2993 | 2990 | 2989 | 2986 | 2987 | 2988 | 2982 | 2983 | 2984 | 2985 | 2979 | 2980 | 2976 | 2977 | 2974 | 2973 | 2970 | 2971 | 2967 | 2968 | 2969 | 2966 | 2964 | 2965 | 2963 | 2961 | 2962 | 2960 | 2958 | 2952 | 2953 | 2954 | 2955 | 2956 | 2950 | 2951 | 2948 | 2949 | 2945 | 2946 | 2947 | 2944 | 2943 | 2939 | 2940 | 2941 | 2942 | 2937 | 2938 | 2936 | 2935 | 2929 | 2930 | 2931 | 2932 | 2933 | 2934 | 2928 | 2927 | 2925 | 2926 | 2921 | 2922 | 2923 | 2924 | 2919 | 2920 | 2917 | 2918 | 2915 | 2916 | 2913 | 2914 | 2912 | 2911 | 2910 | 2909 | 2907 | 2908 | 2906 | 2905 | 2903 | 2904 | 2900 | 2899 | 2898 | 2893 | 2894 | 2895 | 2896 | 2897 | 2890 | 2891 | 2892 | 2887 | 2888 | 2889 | 2885 | 2882 | 2883 | 2884 | 2880 | 2881 | 2878 | 2877 | 2872 | 2873 | 2874 | 2875 | 2876 | 2871 | 2868 | 2869 | 2870 | 2866 | 2867 | 2865 | 2864 | 2862 | 2863 | 2861 | 2860 | 2858 | 2859 | 2856 | 2857 | 2854 | 2855 | 2853 | 2852 | 2848 | 2849 | 2850 | 2847 | 2845 | 2846 | 2843 | 2842 | 2840 | 2841 | 2839 | 2838 | 2837 | 2836 | 2835 | 2833 | 2834 | 2832 | 2831 | 2828 | 2829 | 2827 | 2826 | 2825 | 2824 | 2822 | 2823 | 2820 | 2821 | 2819 | 2816 | 2815 | 2814 | 2813 | 2812 | 2811 | 2793 | 2794 | 2795 | 2796 | 2797 | 2798 | 2799 | 2800 | 2801 | 2802 | 2803 | 2804 | 2805 | 2806 | 2807 | 2808 | 2809 | 2810 | 2791 | 2792 | 2790 | 2787 | 2788 | 2784 | 2785 | 2786 | 2781 | 2782 | 2780 | 2777 | 2778 | 2779 | 2776 | 2775 | 2774 | 2772 | 2771 | 2769 | 2770 | 2768 | 2767 | 2766 | 2764 | 2765 | 2762 | 2763 | 2761 | 2760 | 2759 | 2758 | 2756 | 2752 | 2753 | 2754 | 2755 | 2750 | 2751 | 2748 | 2749 | 2747 | 2745 | 2746 | 2742 | 2743 | 2740 | 2741 | 2739 | 2737 | 2738 | 2736 | 2735 | 2734 | 2733 | 2732 | 2729 | 2730 | 2731 | 2728 | 2727 | 2726 | 2723 | 2724 | 2725 | 2722 | 2719 | 2720 | 2721 | 2718 | 2716 | 2715 | 2714 | 2713 | 2712 | 2711 | 2709 | 2708 | 2706 | 2707 | 2704 | 2705 | 2703 | 2702 | 2700 | 2693 | 2694 | 2695 | 2696 | 2697 | 2698 | 2699 | 2692 | 2690 | 2691 | 2689 | 2688 | 2687 | 2686 | 2685 | 2684 | 2683 | 2680 | 2681 | 2682 | 2678 | 2679 | 2677 | 2676 | 2675 | 2674 | 2673 | 2672 | 2671 | 2670 | 2669 | 2666 | 2668 | 2664 | 2665 | 2662 | 2663 | 2660 | 2661 | 2656 | 2657 | 2658 | 2659 | 2655 | 2654 | 2653 | 2652 | 2649 | 2650 | 2651 | 2646 | 2647 | 2648 | 2643 | 2644 | 2641 | 2642 | 2639 | 2640 | 2637 | 2638 | 2635 | 2636 | 2633 | 2634 | 2631 | 2632 | 2630 | 2629 | 2627 | 2628 | 2624 | 2626 | 2621 | 2622 | 2623 | 2618 | 2619 | 2617 | 2614 | 2615 | 2616 | 2613 | 2612 | 2607 | 2608 | 2609 | 2611 | 2606 | 2605 | 2602 | 2603 | 2604 | 2600 | 2601 | 2599 | 2598 | 2597 | 2595 | 2596 | 2591 | 2592 | 2593 | 2594 | 2585 | 2586 | 2587 | 2588 | 2589 | 2590 | 2584 | 2583 | 2582 | 2581 | 2578 | 2580 | 2576 | 2577 | 2573 | 2574 | 2575 | 2572 | 2571 | 2566 | 2567 | 2569 | 2570 | 2563 | 2565 | 2562 | 2561 | 2560 | 2558 | 2559 | 2557 | 2556 | 2554 | 2555 | 2551 | 2552 | 2548 | 2549 | 2550 | 2547 | 2545 | 2546 | 2542 | 2543 | 2544 | 2540 | 2541 | 2539 | 2537 | 2536 | 2533 | 2534 | 2535 | 2531 | 2532 | 2530 | 2528 | 2525 | 2526 | 2527 | 2522 | 2523 | 2521 | 2519 | 2520 | 2518 | 2517 | 2516 | 2515 | 2514 | 2511 | 2512 | 2509 | 2510 | 2508 | 2506 | 2507 | 2505 | 2504 | 2503 | 2502 | 2501 | 2499 | 2490 | 2494 | 2495 | 2496 | 2497 | 2498 | 2489 | 2488 | 2487 | 2486 | 2485 | 2484 | 2483 | 2482 | 2481 | 2479 | 2480 | 2478 | 2474 | 2475 | 2476 | 2477 | 2472 | 2473 | 2471 | 2470 | 2465 | 2466 | 2467 | 2468 | 2469 | 2464 | 2461 | 2460 | 2459 | 2458 | 2457 | 2454 | 2455 | 2456 | 2451 | 2452 | 2453 | 2449 | 2450 | 2447 | 2448 | 2442 | 2443 | 2444 | 2445 | 2446 | 2440 | 2441 | 2439 | 2436 | 2437 | 2438 | 2434 | 2435 | 2433 | 2432 | 2429 | 2430 | 2431 | 2425 | 2426 | 2427 | 2428 | 2422 | 2423 | 2424 | 2421 | 2417 | 2418 | 2419 | 2420 | 2416 | 2415 | 2412 | 2411 | 2410 | 2408 | 2409 | 2407 | 2406 | 2405 | 2403 | 2404 | 2402 | 2401 | 2400 | 2399 | 2398 | 2397 | 2396 | 2395 | 2394 | 2392 | 2393 | 2390 | 2389 | 2387 | 2386 | 2385 | 2384 | 2383 | 2380 | 2375 | 2376 | 2377 | 2378 | 2379 | 2374 | 2373 | 2372 | 2371 | 2369 | 2370 | 2366 | 2368 | 2361 | 2362 | 2363 | 2364 | 2365 | 2360 | 2359 | 2355 | 2356 | 2357 | 2354 | 2353 | 2350 | 2351 | 2348 | 2349 | 2346 | 2347 | 2344 | 2345 | 2343 | 2342 | 2341 | 2337 | 2339 | 2340 | 2335 | 2336 | 2334 | 2333 | 2328 | 2329 | 2330 | 2331 | 2332 | 2327 | 2326 | 2323 | 2324 | 2325 | 2322 | 2321 | 2316 | 2317 | 2318 | 2319 | 2320 | 2314 | 2315 | 2311 | 2312 | 2313 | 2309 | 2308 | 2306 | 2307 | 2304 | 2305 | 2303 | 2299 | 2300 | 2301 | 2297 | 2294 | 2295 | 2296 | 2292 | 2278 | 2279 | 2280 | 2282 | 2283 | 2284 | 2285 | 2286 | 2287 | 2288 | 2289 | 2290 | 2273 | 2274 | 2275 | 2276 | 2277 | 2271 | 2270 | 2269 | 2266 | 2265 | 2263 | 2264 | 2260 | 2261 | 2259 | 2258 | 2257 | 2255 | 2256 | 2254 | 2250 | 2252 | 2249 | 2247 | 2248 | 2246 | 2242 | 2243 | 2245 | 2239 | 2240 | 2241 | 2235 | 2236 | 2237 | 2238 | 2234 | 2233 | 2232 | 2231 | 2230 | 2229 | 2225 | 2226 | 2224 | 2222 | 2223 | 2220 | 2221 | 2218 | 2219 | 2216 | 2217 | 2214 | 2215 | 2213 | 2211 | 2212 | 2210 | 2209 | 2208 | 2207 | 2206 | 2205 | 2203 | 2204 | 2202 | 2201 | 2199 | 2200 | 2198 | 2197 | 2195 | 2196 | 2194 | 2192 | 2193 | 2191 | 2189 | 2190 | 2188 | 2186 | 2187 | 2185 | 2184 | 2182 | 2183 | 2180 | 2178 | 2179 | 2176 | 2177 | 2172 | 2173 | 2174 | 2175 | 2171 | 2166 | 2167 | 2169 | 2170 | 2165 | 2156 | 2157 | 2158 | 2159 | 2161 | 2162 | 2164 | 2153 | 2154 | 2155 | 2151 | 2150 | 2148 | 2149 | 2142 | 2143 | 2144 | 2145 | 2146 | 2147 | 2140 | 2141 | 2138 | 2139 | 2136 | 2137 | 2135 | 2129 | 2130 | 2131 | 2132 | 2133 | 2134 | 2128 | 2127 | 2126 | 2125 | 2124 | 2121 | 2122 | 2123 | 2118 | 2117 | 2115 | 2116 | 2114 | 2113 | 2112 | 2111 | 2109 | 2108 | 2107 | 2106 | 2104 | 2105 | 2101 | 2102 | 2103 | 2099 | 2100 | 2096 | 2094 | 2095 | 2093 | 2092 | 2091 | 2089 | 2090 | 2088 | 2087 | 2086 | 2085 | 2084 | 2082 | 2083 | 2081 | 2078 | 2079 | 2080 | 2076 | 2077 | 2073 | 2074 | 2075 | 2071 | 2069 | 2066 | 2067 | 2068 | 2064 | 2060 | 2061 | 2062 | 2059 | 2057 | 2058 | 2052 | 2053 | 2054 | 2055 | 2056 | 2049 | 2050 | 2051 | 2048 | 2047 | 2046 | 2042 | 2043 | 2044 | 2045 | 2040 | 2039 | 2038 | 2036 | 2035 | 2029 | 2030 | 2031 | 2033 | 2034 | 2027 | 2024 | 2025 | 2026 | 2017 | 2018 | 2019 | 2020 | 2021 | 2022 | 2016 | 2015 | 2014 | 2013 | 2010 | 2011 | 2012 | 2008 | 2009 | 2007 | 2001 | 2002 | 2003 | 2004 | 2005 | 1993 | 1995 | 1998 | 2000 | 1990 | 1991 | 1987 | 1988 | 1986 | 1983 | 1984 | 1976 | 1977 | 1978 | 1979 | 1980 | 1981 | 1974 | 1975 | 1973 | 1972 | 1970 | 1968 | 1969 | 1967 | 1966 | 1965 | 1964 | 1962 | 1961 | 1959 | 1960 | 1955 | 1956 | 1957 | 1954 | 1952 | 1953 | 1950 | 1951 | 1948 | 1947 | 1946 | 1944 | 1945 | 1940 | 1941 | 1942 | 1943 | 1939 | 1934 | 1935 | 1936 | 1937 | 1938 | 1932 | 1933 | 1931 | 1930 | 1928 | 1927 | 1922 | 1923 | 1924 | 1925 | 1926 | 1916 | 1918 | 1919 | 1920 | 1921 | 1915 | 1914 | 1906 | 1907 | 1908 | 1909 | 1910 | 1911 | 1912 | 1913 | 1902 | 1904 | 1905 | 1895 | 1896 | 1897 | 1899 | 1900 | 1901 | 1891 | 1893 | 1894 | 1890 | 1888 | 1889 | 1887 | 1885 | 1882 | 1883 | 1884 | 1874 | 1875 | 1876 | 1877 | 1878 | 1879 | 1870 | 1871 | 1872 | 1873 | 1868 | 1867 | 1866 | 1865 | 1864 | 1858 | 1859 | 1860 | 1861 | 1862 | 1863 | 1854 | 1855 | 1850 | 1851 | 1852 | 1848 | 1849 | 1846 | 1847 | 1843 | 1844 | 1845 | 1842 | 1831 | 1832 | 1833 | 1834 | 1835 | 1836 | 1838 | 1839 | 1840 | 1841 | 1828 | 1829 | 1830 | 1827 | 1826 | 1825 | 1823 | 1824 | 1818 | 1819 | 1820 | 1821 | 1822 | 1817 | 1815 | 1816 | 1814 | 1812 | 1811 | 1809 | 1810 | 1807 | 1806 | 1805 | 1804 | 1803 | 1802 | 1796 | 1797 | 1798 | 1799 | 1800 | 1801 | 1792 | 1793 | 1794 | 1791 | 1790 | 1789 | 1788 | 1786 | 1785 | 1781 | 1782 | 1783 | 1784 | 1780 | 1779 | 1776 | 1775 | 1772 | 1773 | 1770 | 1769 | 1768 | 1767 | 1763 | 1765 | 1766 | 1762 | 1760 | 1761 | 1757 | 1758 | 1759 | 1755 | 1749 | 1750 | 1751 | 1752 | 1753 | 1754 | 1748 | 1747 | 1745 | 1744 | 1742 | 1743 | 1740 | 1736 | 1737 | 1735 | 1733 | 1732 | 1729 | 1722 | 1723 | 1716 | 1717 | 1718 | 1715 | 1714 | 1712 | 1713 | 1711 | 1710 | 1709 | 1708 | 1706 | 1705 | 1699 | 1700 | 1701 | 1702 | 1703 | 1704 | 1693 | 1694 | 1695 | 1696 | 1697 | 1692 | 1687 | 1690 | 1691 | 1685 | 1686 | 1683 | 1684 | 1682 | 1681 | 1679 | 1677 | 1678 | 1675 | 1674 | 1671 | 1672 | 1669 | 1668 | 1665 | 1666 | 1667 | 1663 | 1662 | 1659 | 1658 | 1657 | 1654 | 1655 | 1656 | 1650 | 1647 | 1648 | 1649 | 1638 | 1637 | 1636 | 1635 | 1628 | 1623 | 1625 | 1626 | 1627 | 1618 | 1619 | 1622 | 1614 | 1615 | 1616 | 1617 | 1613 | 1603 | 1606 | 1607 | 1608 | 1609 | 1611 | 1612 | 1591 | 1592 | 1593 | 1594 | 1595 | 1596 | 1597 | 1598 | 1599 | 1600 | 1602 | 1578 | 1579 | 1580 | 1581 | 1582 | 1583 | 1584 | 1585 | 1586 | 1587 | 1588 | 1589 | 1590 | 1576 | 1577 | 1575 | 1574 | 1573 | 1288 | 1570 | 1565 | 1566 | 1567 | 1568 | 1564 | 1560 | 1559 | 1555 | 1556 | 1557 | 1558 | 1551 | 1553 | 1554 | 1548 | 1549 | 1550 | 1547 | 1545 | 1546 | 1543 | 1544 | 1537 | 1538 | 1542 | 1533 | 1531 | 1529 | 1528 | 1525 | 1526 | 1527 | 1523 | 1524 | 1521 | 1520 | 1517 | 1518 | 1519 | 1515 | 1516 | 1509 | 1510 | 1511 | 1504 | 1505 | 1506 | 1507 | 1508 | 1499 | 1500 | 1501 | 1502 | 1503 | 1497 | 1498 | 1493 | 1494 | 1495 | 1496 | 1489 | 1488 | 1487 | 1485 | 1484 | 1479 | 1481 | 1483 | 1621 | 1477 | 1476 | 1472 | 1473 | 1471 | 1470 | 1468 | 1469 | 1467 | 1454 | 1457 | 1458 | 1459 | 1460 | 1461 | 1462 | 1463 | 1452 | 1451 | 1446 | 1447 | 1448 | 1449 | 1450 | 1442 | 1443 | 1432 | 1435 | 1436 | 1437 | 1439 | 1396 | 1399 | 1401 | 1402 | 1403 | 1404 | 1405 | 1407 | 1408 | 1409 | 1410 | 1411 | 1412 | 1413 | 1414 | 1418 | 1419 | 1420 | 1421 | 1422 | 1423 | 1424 | 1425 | 1426 | 1427 | 1429 | 1430 | 1341 | 1342 | 1343 | 1344 | 1391 | 1392 | 1393 | 1394 | 1339 | 1340 | 1337 | 1329 | 1330 | 1331 | 1332 | 1333 | 1335 | 1328 | 1327 | 1321 | 1322 | 1323 | 1324 | 1325 | 1320 | 1301 | 1302 | 1303 | 1304 | 1305 | 1306 | 1307 | 1308 | 1309 | 1310 | 1311 | 1312 | 1313 | 1314 | 1315 | 1297 | 1298 | 1299 | 1300 | 1291 | 1292 | 1293 | 1295 | 1296 | 1290 | 1280 | 1281 | 1282 | 1285 | 1286 | 1287 | 1279 | 1276 | 1277 | 1278 | 1275 | 1264 | 1265 | 1266 | 1268 | 1269 | 1270 | 1271 | 1272 | 1273 | 1261 | 1262 | 1259 | 1260 | 1257 | 1258 | 1255 | 1254 | 1252 | 1250 | 1249 | 1247 | 1243 | 1244 | 1245 | 1246 | 1241 | 1242 | 1240 | 1238 | 1239 | 1237 | 1236 | 1235 | 1231 | 1232 | 1233 | 1234 | 1228 | 1229 | 1230 | 1224 | 1225 | 1226 | 1223 | 1220 | 1221 | 1222 | 1215 | 1216 | 1217 | 1218 | 1211 | 1212 | 1213 | 1214 | 1209 | 1210 | 1208 | 1202 | 1204 | 1205 | 1206 | 1200 | 1201 | 1199 | 1196 | 1198 | 1192 | 1193 | 1189 | 1190 | 1191 | 1185 | 1178 | 1179 | 1182 | 1184 | 1166 | 1167 | 1168 | 1169 | 1171 | 1173 | 1174 | 1164 | 1163 | 1153 | 1154 | 1155 | 1156 | 1157 | 1158 | 1159 | 1160 | 1161 | 1151 | 1152 | 1147 | 1148 | 1149 | 1146 | 1142 | 1143 | 1144 | 1145 | 1138 | 1139 | 1140 | 1136 | 1133 | 1134 | 1135 | 1132 | 629 | 1130 | 1131 | 1129 | 1123 | 1124 | 1125 | 1126 | 1127 | 1128 | 1122 | 1121 | 1120 | 1119 | 1116 | 1117 | 1118 | 1115 | 1114 | 1109 | 1111 | 1112 | 1113 | 1107 | 1106 | 1099 | 1100 | 1101 | 1102 | 1103 | 1098 | 1094 | 1095 | 1097 | 1093 | 1091 | 1092 | 1089 | 1090 | 1088 | 1085 | 1086 | 1081 | 1082 | 1078 | 1079 | 1080 | 1076 | 1077 | 1075 | 1074 | 743 | 1072 | 1073 | 1070 | 1071 | 1069 | 1068 | 1067 | 1057 | 1058 | 1059 | 1060 | 1061 | 1062 | 1063 | 1064 | 1065 | 1066 | 1055 | 730 | 1047 | 1048 | 1049 | 1050 | 1051 | 1052 | 1053 | 1042 | 1043 | 1044 | 1045 | 1046 | 1036 | 1037 | 1038 | 1039 | 1040 | 1041 | 1034 | 1035 | 910 | 1032 | 935 | 1030 | 1031 | 1026 | 1027 | 1028 | 1029 | 1024 | 1025 | 1023 | 1021 | 1022 | 1018 | 1019 | 1020 | 1017 | 684 | 1016 | 1015 | 890 | 1014 | 1011 | 1012 | 1013 | 1010 | 1009 | 1008 | 1007 | 660 | 1006 | 690 | 1005 | 1002 | 1003 | 997 | 999 | 1000 | 1001 | 996 | 995 | 994 | 987 | 988 | 989 | 990 | 991 | 992 | 984 | 985 | 986 | 431 | 983 | 982 | 979 | 980 | 981 | 961 | 977 | 978 | 975 | 976 | 972 | 974 | 969 | 970 | 971 | 968 | 911 | 967 | 817 | 850 | 853 | 658 | 659 | 439 | 966 | 964 | 962 | 963 | 960 | 958 | 959 | 957 | 954 | 955 | 956 | 952 | 953 | 949 | 950 | 951 | 947 | 948 | 946 | 945 | 944 | 943 | 942 | 941 | 938 | 936 | 937 | 934 | 931 | 932 | 933 | 752 | 292 | 815 | 816 | 819 | 316 | 832 | 839 | 846 | 847 | 854 | 855 | 863 | 864 | 865 | 362 | 879 | 888 | 891 | 918 | 689 | 716 | 722 | 724 | 741 | 744 | 746 | 749 | 750 | 929 | 927 | 928 | 925 | 926 | 924 | 153 | 923 | 919 | 920 | 921 | 916 | 914 | 912 | 908 | 909 | 905 | 906 | 464 | 354 | 904 | 878 | 900 | 893 | 894 | 895 | 896 | 897 | 892 | 898 | 899 | 889 | 351 | 885 | 886 | 880 | 881 | 883 | 884 | 667 | 874 | 875 | 361 | 930 | 940 | 430 | 434 | 873 | 825 | 826 | 828 | 829 | 844 | 845 | 849 | 852 | 856 | 857 | 858 | 859 | 860 | 870 | 697 | 764 | 862 | 861 | 818 | 851 | 663 | 830 | 831 | 833 | 834 | 835 | 836 | 838 | 840 | 842 | 843 | 824 | 837 | 822 | 820 | 801 | 810 | 811 | 812 | 814 | 628 | 656 | 657 | 661 | 664 | 665 | 666 | 668 | 669 | 670 | 674 | 675 | 677 | 680 | 681 | 682 | 683 | 685 | 686 | 687 | 688 | 691 | 692 | 693 | 694 | 696 | 698 | 699 | 700 | 701 | 702 | 703 | 704 | 705 | 713 | 459 | 717 | 719 | 720 | 721 | 725 | 729 | 731 | 734 | 736 | 737 | 740 | 748 | 751 | 754 | 755 | 756 | 757 | 758 | 759 | 760 | 761 | 762 | 711 | 813 | 809 | 808 | 803 | 804 | 805 | 364 | 802 | 800 | 798 | 796 | 797 | 795 | 791 | 792 | 793 | 794 | 461 | 790 | 787 | 788 | 770 | 771 | 772 | 773 | 774 | 775 | 777 | 782 | 784 | 768 | 769 | 767 | 765 | 766 | 626 | 726 | 727 | 728 | 710 | 706 | 295 | 444 | 484 | 652 | 654 | 655 | 643 | 646 | 647 | 648 | 649 | 650 | 630 | 631 | 633 | 634 | 635 | 638 | 639 | 640 | 564 | 578 | 579 | 582 | 583 | 584 | 587 | 588 | 590 | 591 | 592 | 593 | 594 | 595 | 596 | 597 | 598 | 599 | 600 | 601 | 602 | 603 | 604 | 605 | 606 | 607 | 608 | 609 | 610 | 611 | 613 | 614 | 615 | 616 | 617 | 618 | 619 | 620 | 623 | 438 | 442 | 443 | 447 | 448 | 455 | 465 | 466 | 472 | 473 | 481 | 482 | 483 | 576 | 575 | 562 | 532 | 535 | 537 | 539 | 541 | 543 | 545 | 547 | 551 | 553 | 555 | 513 | 514 | 515 | 516 | 517 | 518 | 519 | 520 | 521 | 522 | 523 | 524 | 525 | 526 | 527 | 528 | 530 | 500 | 501 | 502 | 503 | 504 | 505 | 506 | 507 | 508 | 509 | 511 | 487 | 488 | 489 | 491 | 492 | 495 | 496 | 499 | 458 | 456 | 360 | 294 | 293 | 415 | 416 | 404 | 402 | 397 | 398 | 401 | 396 | 377 | 386 | 372 | 369 | 368 | 358 | 344 | 353 | 355 | 321 | 322 | 325 | 319 | 257 | 8 | 13 | 14 | 271 | 272 | 33 | 289 | 34 | 35 | 296 | 44 | 45 | 86 | 98 | 100 | 106 | 117 | 139 | 145 | 159 | 182 | 183 | 184 | 185 | 210 | 211 | 212 | 216 | 222 | 223 | 235 | 239 | 240 | 243 | 246 | 248 | 250 | 3587 | 3590 | 3160

Lithium and the dramatic surface of AMACO PC-32 Albany Slip Brown

Left is G3933A; right is AMACO PC-32 Albany Slip Brown. PC-32 shows much greater movement and a stronger contrast between creamy areas and rich brown. AMACO identifies lithium carbonate in this product, and our own tests show that adding lithium carbonate to a related glaze can greatly increase melt fluidity and transform its appearance. That supports lithium’s importance here, although it does not reveal AMACO’s base recipe or lithium percentage.

Where PC-32 collects more thickly, it develops a lighter, more opaque appearance; over raised contours, it thins and breaks brown. Crystallization may contribute to the cream-colored areas, but opacity as a product of phase separation is another possible mechanism. This raises an interesting development challenge: Can a lithium-free formulation reproduce both the flowing melt and the distinctive cream–brown separation? With the cost of lithium materials it is easy to imagine development work is being done.

Lithium albany brown glaze

Related Pictures

Add 6% lithium carbonate to an Alberta Slip glaze:

And this happens!


Alberta slip + lithium carbonate glaze

This picture has its own page with more detail, click here to see it.

Left is G3933A, it is an 80:20 mix of G2934 matte and G2926B glossy cone 6 base recipes (plus a mix of iron oxide, tin oxide and rutile). The body is Plainsman Coffee Clay. Because of repeated issues with crawling, a project was started to create the same effect using Alberta Slip to supply as much of the chemistry as possible. Along that road, the opportunity arose to add lithium (to duplicate Amaco PC-32, a classic Albany/Lithium recipe). The glaze on the mug on the right is G3933G1, it adds 6% lithium carbonate. Lithium is a super powerful melter, turning this into a very reactive glaze! However, there is a down side: To make a 500ml jar of DIY brushing glaze, in 2023, required about $7 worth of lithium carbonate.

Lithium is no longer affordable for ceramics.

Yet in many cases it seems indispensable


This picture has its own page with more detail, click here to see it.

The crystals that form as this cone 6 fluid-melt glaze solidifies are one of the minerals in the recipe: Spodumene. Actually β-spodumene. But it is so expensive, and there is 42% here! What would it take to reduce the cost of making this glaze ($52/kg in 2026)? Another flux could certainly make it just as melt-fluid, but it would not grow spodumene crystals.

β-spodumene is Li2O - Al2O3 - 4SiO2 So the 0.22 Li2O in this glaze would require 0.22 Al2O3 and 0.88 SiO2 to crystallize as a β-spodumene-type lithium aluminosilicate. The glaze contains 0.24 Al2O3 and 1.41 SiO2. There is almost exactly enough lithium to combine with nearly all of the alumina as β-spodumene. The 2% rutile supplies TiO2; it acts as a nucleating agent. Replacing Li2O with another flux could maintain the melt fluidity, but Na2O, K2O or B2O3 cannot simply take the place of Li2O in β-spodumene.

It is possible that less spodumene could still do this. That could be tested by reducing Li2O to 0.1 and increasing Na2O to 0.23 (while maintaining the other oxides as-is). B2O3 could also be tried (it has a far lower thermal expansion). Of course, effecting changes in specific oxides requires some glaze chemistry.

Links

Materials Lithium Carbonate
A powerful melter very valuable in ceramic glazes. It is 40% Li2O and has an LOI of 60% (lost as CO2 on firing). This material in now incredibly expensive.
Materials Albany Slip
A pure low plasticity clay that, by itself, melted to a glossy dark brown glaze at cone 10R. It was a popular glaze ingredient for many decades.
Glossary Reactive Glazes
In ceramics, reactive glazes have variegated surfaces that are a product of more melt fluidity and the presence of opacifiers, crystallizers and phase changers.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy