In a clay body: In a clay body: Compare the original body with one containing the proposed replacement using SHAB test bars fired together. Adjust the replacement percentage to approach the original absorption and firing shrinkage (and fired color, deformation and glaze fit). Nepheline syenite or a suitable soda feldspar may achieve the required maturity at a lower percentage.
In a glaze: Start by matching KNaO—the combined molar amounts of K2O and Na2O. This gives more freedom to use available feldspars without requiring an exact match of potassium and sodium separately. Confirm the result by firing tests. The following are practical starting points, not fixed percentage rules:

This picture has its own page with more detail, click here to see it.
The chemistry for Custer Feldspar has been updated in the materials at Digitalfire and Insight-live. Until now, the Pacer-published values have been used, but at Ron Roy's request, this has been changed (see the link to his article below). The average of assays done from 2000 to 2012 has been used for the chemistry. The material name has been changed to "Custer Feldspar (post-2000)". However, Insight-live will still find it in recipes when needing its chemistry, since "Custer Feldspar" has been included as an alternate name. The old material's name has been changed to "Custer Feldspar (pre-2000)".
In this image, you can see the material chemistries on the right and each of them being used in a one-material recipe on the left. To verify they are calculating correctly, the calculation of each has been set to formula plus analysis.
If you have defined your own material for this (typically done to set a cost), everything should still work correctly (using your chemistry if you provided it).

This picture has its own page with more detail, click here to see it.
The speckled iron stoneware recipes I created in the past had a major problem: Color variation as a product of natural material changes. To illustrate, zoom in on the bare clay bases on these mugs. The differences in the variegated light and dark color patching is a product of differences in fired maturity. Small differences which I can measure as porosity (water absorption on an SHAB test).
The solution is to create a more refractory base body and add some feldspar to reduce its porosity to 3%. Why? The feldspar percentage can then be tuned to compensate for material changes in each production mix. These mugs illustrate. The base recipe for them is a two-part mix of red stoneware and two buff fireclays.
The next move: I want the more plastic base of #3, but with less fired maturity. It is just a matter of testing to reduce the Nepheline percentage.

This picture has its own page with more detail, click here to see it.
My G2571A and G1947U cone 10R glaze recipes are both in use in Ecuador. One user has been importing Custer feldspar, but now needs to substitute a local one. That material is much higher in SiO2 and much lower in Al2O3 and KNaO (so a pound-for-pound substitution is likely not going to work). Here is how I did the chemistry. It turned out to be a matter of increasing the new feldspar to match the KNaO (which also matched the Al2O3) and then reducing the silica to match the SiO2. The amount by which I had to change the feldspar is a testament to how different the chemistry of these materials can be from country to country.
If you do this calculation, please note the following: In August 2026 the name for Custer Feldspar was changed to "Custer Feldspar (post-2000)" (both here and in the Insight-live reference materials). There is also one for "Custer Feldspar (pre-2000)".
| Hazards |
Feldspar
Feldspars are abundant and varied in nature. They contain small amounts of quartz (while nepheline syenite does not). |
| Materials |
Custer Feldspar (pre-2000)
The most common potash feldspar used in ceramics in North America, a standard for many decades, but no longer available. Its chemistry shifted around 2000. |