0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Rate | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Interaction | Oxide Molecular Formula | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Molecular Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Calculated Thermal Expansion

Calculation of the thermal expansion of glazes is a very useful comparative glaze-fit tool. But it’s not a laboratory measurement.

Key phrases linking here: calculated thermal expansion, calculated coe - Learn more

Details

Calculated thermal expansion is one of the most useful numbers in glaze chemistry—but it is important to understand what it is, and what it is not.

Digitalfire Insight-live calculates a coefficient of thermal expansion (CTE) from the oxide analysis of a glaze. Using the traditional weight-percent method, the amount of each oxide is multiplied by an expansion factor assigned to that oxide and the contributions are summed. If the analysis is not already normalized to 100%, it is normalized as part of the calculation. Insight-live also performs a secondary calculation using mole percentages and the corresponding molar expansion factors.

The default oxide expansion factors are found on the Preferences page and can be changed. For example, the West & Gerrow weight-percent factors used by Digitalfire include SiO2=0.035 and K2O=0.331. These numbers are scaled for convenience so that a typical glaze calculates to a familiar single-digit number such as 6.3 or 7.0. Laboratory CTEs are commonly expressed as ×10^-6/°C or ×10^-6/K, but the number calculated by Insight-live should be regarded primarily as a comparative value, not as a laboratory measurement. That distinction is important.

Where do the oxide expansion factors come from?

It is tempting to imagine that each oxide has its own inherent thermal expansion and that a glaze calculation simply adds those expansions together. That is not really what is happening.

The coefficients used in these calculations are empirical contribution factors derived from observations of glasses and glazes having different compositions. Hall, for example, developed an additive calculation from measurements of 118 glasses and glazes. Other researchers developed other coefficient sets, sometimes producing substantially different numbers.

The model assumes that the expansion of a glass can be approximated by adding the contributions associated with its constituent oxides. This works surprisingly well within many related families of glasses, but it is still an approximation. Oxides interact to build the glass structure, so their effects are not completely independent or necessarily linear.

Different published coefficient sets therefore give different calculated values. Some include oxides that others omit. Some use weight percentage and others use molar proportions. These factors must be used with the calculation method for which they were intended.

At Digitalfire, we compared measured thermal expansions of hundreds of frits with values calculated using various coefficient sets. We found the West & Gerrow values particularly useful - not necessarily because they predicted the absolute laboratory CTE best, but because they produced useful comparative relationships between compositions. That comparative role is the key to making calculated thermal expansion useful.

Calculated CTE works best within a glaze system

Calculated thermal expansion values are much more reliable for predicting direction of change than absolute expansion. They work best when comparing closely related glazes. Suppose you have a balanced cone 6 transparent glaze that crazes. If you alter the recipe so that K2O and Na2O decrease, MgO increases and SiO2 increases, and the calculated expansion falls from 7.0 to 6.5, there is a good probability that the fired glaze will also have a lower thermal expansion. That is staying “within a system.” The comparison becomes progressively less reliable as you move outside that system - for example, by introducing new oxides, changing significantly from raw materials to frits, changing firing temperature, producing crystallization or phase separation, or altering the degree to which materials actually dissolve into the melt.

Calculated expansion is least useful when applied to an unfamiliar glaze having no fired history at all. A value of 6.5 does not, by itself, tell you whether that glaze will fit a particular clay body. The number becomes useful when you know that this glaze at 7.0 crazes and want to calculate a version at 6.7 or 6.5 and test it.

Oxide effects are not always linear

The simple additive calculation assumes that the contribution of an oxide changes proportionally with its amount. Real glasses are more complicated. Changes in B2O3, Li2O, SiO2 and other oxides can restructure a glass in ways that make their effects composition-dependent. Published expansion models even assign variable coefficients to some oxides depending on composition. Thus the direction predicted by calculation is usually more trustworthy than the exact magnitude of the change. This is another reason experience within a particular glaze family is so valuable. After several calculate-test-adjust cycles, you begin to know what a change from, say, 7.0 to 6.7 actually means for that glaze and body combination.

A glaze must actually become the glass being calculated

The calculation is fundamentally a glass-composition model. It therefore becomes less representative when the fired glaze is not a homogeneous glass.

Frits begin as homogeneous glasses and generally melt predictably. Raw glaze materials, by contrast, can contain particles of quartz, feldspar, clay minerals, zircon, rutile and other phases having very different decomposition and dissolution behaviours.

If firing produces a well-melted homogeneous glass, much of that mineralogical history disappears and the calculated oxide chemistry becomes highly relevant. But if substantial particles remain undissolved, or if crystals precipitate during cooling, the fired glaze is no longer simply the homogeneous glass assumed by the calculation.

Particle size can therefore matter. Fine silica, for example, generally dissolves into a glaze melt more readily than coarse silica. Two recipes having identical calculated chemistry can consequently fire differently if one leaves significantly more residual quartz than the other.

Zircon is an obvious example. Much of it normally remains as discrete crystalline particles suspended in the glaze. Its effect on the thermal expansion of the fired coating is therefore not equivalent to simply treating its ZrO2 and SiO2 as if they had dissolved completely into the glass.

Can clay-body expansion be calculated?

Not with this method. More precisely, the thermal expansion of a fired clay body cannot be usefully predicted from its bulk oxide analysis using an additive glaze-expansion calculation. A fired body is not a homogeneous glass. It is a composite of crystalline and glassy phases whose identities and proportions depend on the original minerals, particle sizes and firing history.

Consider SiO2. Two bodies can have exactly the same bulk SiO2 percentage while having very different expansion behaviour. One might contain substantial residual quartz grains. In another, much more of the SiO2 might have entered a feldspathic glass or participated in the formation of other phases.

Quartz is especially important because residual quartz undergoes its α-β inversion near 573°C. Cristobalite, when present, produces another prominent expansion event at much lower temperature. Mullite, feldspathic glass, residual minerals, porosity and microcracking all contribute differently to the overall expansion behaviour.

Thus body expansion is a product not simply of chemistry but of mineralogy plus firing history plus microstructure. Variables such as particle size distribution, mineralogy, quartz content, firing temperature, firing duration, atmosphere and cooling schedule can all change the phase assemblage of the fired body without substantially changing its bulk chemical analysis. That is why calculated glaze chemistry can be so useful while calculated body chemistry cannot predict expansion in the same way.

What does a dilatometer tell us? It measures the dimensional change of an actual fired specimen as temperature changes. That makes it especially valuable for clay bodies.

But even a measured CTE is not a single, immutable property that covers every temperature. The dilatometer actually produces an expansion curve. A reported CTE is normally the average slope of some specified portion of that curve.

That distinction matters greatly for ceramic bodies because quartz and cristobalite transformations can produce pronounced changes in slope. A single number cannot describe all of this behaviour. Measured expansion data are nevertheless extremely useful. If several bodies are measured by the same method over the same temperature range, they can be ranked reliably from lower to higher expansion.

Suppose a glaze crazes on body A. If body B has a somewhat higher thermal expansion over the relevant temperature range, the glaze will normally be placed under greater compression on B and may fit it better. Too much difference in the opposite direction, of course, introduces the possibility of shivering or body failure.

Dilatometry is therefore extremely useful for comparing bodies with bodies and glasses with glasses. What should be avoided is assuming that an uncalibrated calculated glaze value of 6.5 and a laboratory body value of 6.5 are necessarily a matched pair. They were arrived at in completely different ways.

Glaze/body stress also depends on more than CTE alone. Glaze stiffness, thickness, body stiffness, geometry and the temperature at which the glaze becomes rigid enough during cooling to sustain stress all play roles.

How should calculated thermal expansion actually be used? Comparatively. Suppose a glaze crazes and Insight-live calculates its expansion at 7.0. That tells you nothing absolute about whether 7.0 is “good” or “bad.” But you now have a starting point. Adjust the chemistry to lower the calculated expansion. For a badly crazing glaze, you might initially target 6.5. Fire it on the same body using the same schedule and subject it to an appropriate thermal-stress test. If it still crazes, move the calculated value lower. If crazing disappears, test sufficiently to make sure the glaze has not moved too far toward excessive compression and shivering. If the original glaze crazes only after severe thermal stressing, a much smaller calculated change may be enough.

Of course, changing chemistry to control expansion can have side effects. Increasing SiO2 can alter melt fluidity. Trading K2O and Na2O for MgO can change gloss, crystallization and surface character. Changing B2O3 can alter melting behaviour. Successful fit adjustment therefore requires maintaining the other properties of the glaze while moving its expansion in the required direction.

But this is exactly where calculated thermal expansion becomes so valuable. Instead of blindly changing recipes and hoping something works, you can make directed changes, fire tests and build experience correlating calculated movement with actual glaze fit. That is what the number is for.

Related Information

Adding silica will fix crazing, right? Not here.


Thee porcelain mugs, the glaze on two are crazed

This picture has its own page with more detail, click here to see it.

G2926B (center and right) is a clear cone 6 glaze created by simply adding 10% silica to Perkins Studio clear (a glaze that had a slight tendency delay-craze on common porcelains we use). Amazingly that glaze tolerated the silica addition very well, continuing to fire to an ultra gloss crystal clear. That change eliminated the crazing issues on most of our bodies. The cup on the right is one of them, that body is vitreous, near-zero-porosity, and fits most glazes. Why? Because it has 24% silica in the recipe. The center porcelain is also dense and vitreous, but it only has 17% silica, that is why it is crazing this glaze. Then I added 5% more silica to the glaze, it continued to produce an ultra smooth glossy, and applied it to the 17% body on the left. Why did not fix the crazing? That silica addition to the glaze only reduces the calculated expansion from 6.0 to 5.9, clearly not enough to fix the problem. So, the obvious solution seems to be use the porcelain on the right. Are you wondering why adding silica to a body raises its thermal expansion, and adding it to a glaze lowers it? Mineralogy is the reason.

Comparing glaze melt fluidity balls with their chemistries


Three glaze balls melting down into a pool

This picture has its own page with more detail, click here to see it.

Ten-gram GBMF test balls of these three glazes were fired to cone 6 on porcelain tiles. Notice the difference in the degree of melt? Why? You could just say glaze 2 has more frit and feldspar. There is a better explanation, compare these yellow and blue numbers: Glaze 2 and 3 have much more B2O3 (boron, the key flux for cone 6 glazes) and lower SiO2 (silica, it is refractory). But notice that glaze 2 and 3 have the same chemistry, but 3 is melting more? Why? Because of the mineralogy of Gerstley Borate. It release its boron earlier in the firing, getting the melting started sooner. Notice it also stains the glaze amber, it is not as clean as the frit. Notice the calculated thermal expansions: The greater melting of #2 and #3 comes at a cost, their thermal expansions are considerably higher, so they will be more likely to craze. Which of these is the best for functional ware? #1, G2926B (left). Its high SiO2 and enough-but-not-too-much B2O3 make it more durable. And it runs less during firing. And does not craze.

Start glaze chemistry by learning when you don't need it!

A high feldspar glaze is a good example


A runny, amber, crazed glaze

This picture has its own page with more detail, click here to see it.

This reduction celadon is crazing badly. Why? Its chemistry is dominated by feldspar, which supplies lots of K2O and Na2O fluxes. Scores of recipes being traded online contain 50% or more feldspar; they benefit from these powerful fluxes but inherit their high thermal expansion (COE). Many work only because the body happens to have sufficiently high expansion - often aided by significant residual quartz.

Crazing is more than a cosmetic problem in functional pieces. It reduces ware strength and durability, can compromise food safety and turn into a customer complaint. Let's fix it, starting without chemistry:

Secret #5 of crystalline glazes:

They craze. But there is a way to fix that


This picture has its own page with more detail, click here to see it.

The mug on the left, made by Holly McKeen, is a typical cone 10 Grolleg kaolin mullite porcelain (highly vitrified, low in residual quartz). Its glaze is crazed. Crystalline glazes are high in Na2O, making crazing virtually certain. Since most pieces are decorative, crystal glazers just accept this as part of the process. But these are functional mugs, the glaze needs to fit (if only for ware strength).

But what if the thermal expansion of the body could be significantly raised? The body on the right is Crystal Ice, it contains 40% silica (vs 20-25% in a typical porcelain). The percentage of Nepheline has been reduced, lowering vitrification to about 1.5% porosity. As a result, more quartz survives undissolved and less mullite develops, raising the body’s thermal expansion. The result is a body with a much higher thermal expansion, so it can not only relieve the glaze tension but actually put a squeeze on it. There is a downside: These are less resistant to dunting and thermal shock failure during use.

Could the glaze be adjusted instead? Yes. Some of the Na2O could be substituted for Li2O, the latter is also a strong melter but has a much lower thermal expansion. Glaze chemistry could be used to source it from Spodumene (to avoid solubility issues with lithium carbonate). However, zinc-silicate crystalline glazes are very sensitive systems, so the more lithia is introduced the more likely the effect on the firing window, crystal size/density and background clarity.

Insight-Live comparing two recipes:

Glossy and matte cone 6 bases


This picture has its own page with more detail, click here to see it.

Insight-live is calculating the unity formula and mole% formula for the two glazes. Notice how different the formula and mole% are for each (the former compares relative numbers of molecules, the latter their weights). The predominant oxides are very different. The calculation is accurate because all materials in the recipe are linked (clickable to view to the right). Notice the Si:Al Ratio: The matte is much lower. Notice the calculated thermal expansion: The matte is much lower because of its high levels of MgO (low expansion) and low levels of KNaO (high expansion). Notice the LOI: The matte is much higher because it contains significant dolomite.

High thermal expansion talc body cannot be COE-calculated


This picture has its own page with more detail, click here to see it.

Talc is employed in low-fire bodies to raise their thermal expansion (to put the squeeze on glazes to prevent crazing). These dilatometer curves make it very clear just how effective that strategy is! The talc body was fired at cone 04 and the stoneware at cone 6. The former is porous and completely non-vitreous and the latter is semi-vitreous. This demonstrates something else interesting: The impracticality of calculating the thermal expansion of clay bodies based on their oxide chemistry. Talc sources MgO and low fire bodies containing it would calculate to a low thermal expansion. But the opposite happens. Why? Because these bodies are composed of mineral particles loosely sintered together. A few melt somewhat, some change their mineral form, many remain unchanged. The body's COE is the additive sum of the proportionate populations of all the particles. Good luck calculating that!

Match calculated COE to dilatometer-measured body COE? No!


This picture has its own page with more detail, click here to see it.

Why? Firing temperature, schedule and atmosphere affect the result. Dilatometers are only useful when manufacturers monitor bodies AND glazes over time and in the same firing conditions. Calculated values for glazes are only relative (not absolute). The best way to fit glazes to your clay bodies is by testing, evaluation, adjustment and retesting. For example, if a glaze crazes, adjust its recipe to bring the expansion down (your account at Insight-live has the tools and guides to do this). Then fire a glazed piece and thermal stress it (300F-to-ice-water IWCT test). If it still crazes, move it further. If you have a base glossy glaze that fits (and made of the same materials), try comparing its calculated expansion as a guide. Can you calculate body expansion from oxide chemistry? Definitely not, because bodies do not melt.

Two matte mechanisms: One crazes, the other does not


A matte glaze crazing badly

This picture has its own page with more detail, click here to see it.

These two glazes look the same, they are both cone 6 satin mattes. On the same porcelain. But the matteness "mechanism" of the one on the left, VC71, is a low Si:Al ratio melted by zinc and sodium. The mechanism of the one on the right, G2934, is high MgO melted by enough boron to also have plenty of SiO2 and Al2O3. The "baggage" of the mechanism on the left is high thermal expansion and crazing (drastically reducing strength and providing a space for a germ zoo). If your ware develops this your customers will bring it back for replacement. No change in firing will fix this, the body and glaze are not expansion compatible. Period.

Inbound Photo Links


Glaze chemistry explains the crazing
The unexpected reason for this crazing can be seen in the chemistry

Four common lithium carbonate glazes
Lithium carbonate and Gerstley Borate in glazes: What is the best way forward?

Published COE numbers
Are published clay body COE numbers useful to potters?

ChatGPT vs Gemina on crazing glazes
Two ChatBots square off on crazing in 2025

Links

Glossary Thermal Expansion in Ceramic Bodies and Glazes
The co-efficient of thermal expansion of ceramic bodies and glazes determines how well they fit each other and their ability to survive sudden heating and cooling without cracking.
Glossary Oxide System
Glossary Glaze Compression
In ceramics, glazes are under compression when they have a lower thermal expansion than the body. A little compression strengthens ware, too much can weaken and even fracture it.
Glossary Formula Ratios
The ratios of individual or group oxide molecule numbers are indicators of things like fired gloss, durability, melting temperature, balance, tendency to craze, etc.
Glossary Glaze fit
In ceramics, glaze fit refers to the thermal expansion compatibility between glaze and clay body. When the fit is not good the glaze forms a crack pattern or flakes off on contours.
Troubles Glaze Shivering
Ask the right questions to analyse the real cause of glaze shivering. Do not just treat the symptoms, the real cause is thermal expansion mismatch with the body.
Troubles Glaze Crazing
Ask the right questions to analyse the real cause of glaze crazing. Do not just treat the symptoms, the real cause is thermal expansion mismatch with the body.
Oxides MgO - Magnesium Oxide, Magnesia
Articles Understanding Thermal Expansion in Ceramic Glazes
Understanding thermal expansion is the key to dealing with crazing or shivering. There is a rich mans and poor mans way to fit glazes, the latter might be better.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy