0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Rate | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition During Ceramic Firing | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | DTA Test | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | LAS Body | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | LOI-Adjust | Low Temperature Glaze | | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Interaction | Oxide Molecular Formula | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | TGA Test | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Molecular Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Magnesia Matte

Magnesia matte ceramic glazes are “microstructure mattes” while calcia mattes are “crystal mattes”. They have a micro-wrinkle surface that forms from a high viscosity melt and microscopic phase separation, both of which prevent levelling on freezi

Key phrases linking here: magnesia mattes, magnesia matte, mgo matte - Learn more

Details

G2934 cone 6 magnesia matte with a variety of stains added.


Magnesia matte glazes have a characteristic soft satin surface. The mechanism is much more about microstructure rather than crystallization: A micro-wrinkle surface “freezes in” from a high viscosity melt that is too viscous and elastic to fully level on freezing. But it is more complicated, and there are additional mechanisms at play. A microstructure also develops while the melt is stiffening. That process needs time in the glass transition zone (~900–700 °C). Slow cooling stretches that zone out. Submicroscopic phase separation occurs as the glaze cools, the melt becomes less chemically comfortable holding MgO evenly dissolved in the silica-rich glass, and it begins to separate into Mg-rich and an Si-rich glassy phases. These have different viscosities that affect surface levelling, and different refractive indices that affect how light reacts as it hits the boundaries.

But MgO tends to lower the surface tension of the melt; this seems to run counter to the above explanation. However, it seems that magnesia mattes are matte in spite of MgO’s surface-tension behavior, not because of it. As noted, the primary mechanism behind poor levelling during cooling is micro-scale phase change coupled with melt stiffness (the slow cooling enhances this effect, just as it enhances crystallization in calcia mattes; conversely, fast cooling also freezes the melt before the mechanism can develop). There is an additional contributing factor: MgO promotes the formation of magnesium silicate or aluminate nano-crystals (spinels) that are too small to see but large enough to scatter light.

The minimum MgO level in the unity formula of magnesia mattes for pottery is typically 0.3, accompanied by high Al2O3 and a low Si:Al ratio. Controlled cooling is assumed. For matte surfaces with faster cooling, MgO may need to be as high as 0.4 (and SiO2 lower).

In our observations, at high temperatures, a low silica:alumina ratio is necessary to provide a viscous enough melt. Enough KNaO is also needed to get a good glass (since MgO normally enters at the expense of CaO). The KNaO also helps to increase the thermal expansion that may otherwise be too low to fit bodies. Additions of B2O3 can flux the effect down to the cone 6 range (higher KNaO at the expense of CaO can lessen the boron requirements). This works especially well when some of the MgO is sourced from a frit. These frits are remarkable in that they supply a high proportion of the oxide yet melt at a far lower temperature than any MgO-containing natural material blend could do (and have zero-LOI compared to 45% for dolomite). With a significant increase in B2O3 it is even possible to produce the effect at cone 04.

At lower temperatures, there is also recipe level matte mechanism with MgO. Talc, dolomite and magnesium carbonate are all refractory; their resistance to dissolving in the glaze melt can stiffen it and produce a matte surface (although not normally silky). This type of glaze falls outside of this discussion.

At stoneware temperatures, it can be tricky to produce a functional magnesia matte that resists cutlery marking, staining and leaching (one reason why my G2571A recipe is popular). The first challenge is that a viscous melt is a requirement so flux levels must be lower, which introduces the possibility of inadequate melting. Second, lower MgO and higher SiO2 favours better functionality; the more firings can be control-cooled the more these are enabled. Getting a specific surface becomes a question of whether to adapt the firing to the recipe, or the recipe to the firing.

"Dolomite matte" glazes have traditionally been fired around cone 10. It is not the dolomite that produces the matte effect, it is the MgO in the dolomite. But, the name has stuck because dolomite has been the most common source of MgO (talc and magnesium carbonate are others).

Related Information

Calcia vs Magnesia matte:

Different mechanisms and melt fluidities


This picture has its own page with more detail, click here to see it.

This melt flow test was done at cone 6+ (without slow cooling) to demonstrate the difference in melt viscosity between a calcia matte (left G1214Z1) and a magnesia matte (right G2928C, similar to G2934). In simplest terms, the former depends on a fluid melt to provide the needed mobility for tiny crystals to form during cooling; those crystals scatter the light and soften the surface to produce the matte effect. The latter requires a stiffer melt to help prevent levelling during cooling and host phase separation to produce a rippled surface that scatters light.

Step 1 of a speckled dolomite matte at cone 6 oxidation:

This result is good enough to prove it is doable


This picture has its own page with more detail, click here to see it.

I am looking to match the reduction-fired dolomite matte mug on the right, but in cone 6 oxidation. I must duplicate the glaze color and surface character. But more difficult is the speckle size, color, density and edge bleeding. The speckle is the biggest challenge, but I met that by making my own by mixing the body and G2926B glossy glaze 50:50 and adding 10% black stain. Then I slurry it, dry it, fire it in a crucible (which I make from L4404A with an L3693E liner), crush it by hand using my shusher and screen it. I am using G2934 cone 6 magnesia matte as the glaze on this mug on the left. I add 0.5% minus 20 mesh speck to achieve this result. The next step in this project is to sieve out the smallest specks, switch to the G2934 matte glaze in the speckle recipe (the specks are too shiny here), and switch to dark brown stain instead of black. I will also need to control the degree to which the specks bleed at their edges (by adjusting the glaze:body ratio) and tune the degree of matteness (by adjusting cooling speed of the kiln). A small amount of green or blue stain is also needed to match the glaze color. There is no question that an authentic reproduction is possible; methodical testing with good records is the key to accomplishing that.

Tuning the degree of gloss in a colored matte glaze


This picture has its own page with more detail, click here to see it.

Matte glazes have a fragile mechanism. That means the same recipe will be more matte for some people, more glossy for others (due to material, process and firing differences). In addition, certain colors will matte the base more and others will gloss it more. It is therefore critical for matte glaze recipes to have adjustability (a way to change the degree of gloss), both for circumstances and colors. This recipe is Plainsman G2934 base matte with 6% Mason 6600 black stain added. It has been formulated to be on the more matte side of the scale so that, for most people, a simple addition of G2926B (G2926B base recipe) will increase the gloss. That means users need to be prepared to adjust each color of the matte to fine-tune its degree of gloss. Here you can see 5:95, 10:90, 15:85 and 20:80 blends of the matte:gloss recipe bases.

Matte cone 6 glazes have identical chemistry:

But one melts much more. Why?


This picture has its own page with more detail, click here to see it.

These are 10-gram GBMF test balls that we melted on porcelain tiles at cone 4 (top two) and cone 6 (bottom two). They compare the melt fluidity of G2934 (left) and G2934Y (right). The Y version sources its MgO from frit and talc (rather than dolomite). It is a much more fluid melt because the frit is yielding the oxides more readily. But Y has a key benefit: It has a much lower LOI, producing fewer entrained air bubbles and therefore fewer surface defects. And, even though it runs much more, it has the same matte surface! As long as it is applied at normal thickness, the extra melt fluidity does not cause any running. And it has another benefit: fewer cutlery marking issues. It is actually a very durable and practical food surface glaze, having a low thermal expansion that fits almost any body. Although these appear glossy here, on ware they have the identical pleasant silky matte surface.

Matte base glaze cutlery marks.

Add 10% glossy glaze. No marking.


Cutlery marking glaze fixed

This picture has its own page with more detail, click here to see it.

This is G2934Y (a version of the G2934 cone 6 matte base recipe that supplies much of the MgO from a frit instead of dolomite). Like the original, it has a beautiful fine silky matte surface and feels like it would not cutlery mark. But, as you can see on the left, it does! The marks can be cleaned off easily. But still, this is not ideal. The degree of matteness that a glaze has is a product of its chemistry. But can we fix this without doing any chemistry? Yes. By blending in some G2926B clear glossy (90:10 proportions). The result: The marks are gone and the surface is only slightly less matte. This underscores the need to compromise the degree of matteness, on food surfaces, enough to avoid staining and cutlery marking.

The difference between dolomite and calcium carbonate in a glaze


This picture has its own page with more detail, click here to see it.

These glaze cones are fired at cone 6 (without slow cooling) and have the same recipe: 20 Frit 3134, 21 EP Kaolin, 27 calcium carbonate, 32 silica. The difference: The one on the left uses dolomite instead of calcium carbonate. Notice how the MgO from the dolomite mattes the surface (without slow cooling) whereas the CaO from the calcium carbonate produces a brilliant gloss (because it needs slow cooling).

Dolomite bamboo matte glazed cone 10R mug


This picture has its own page with more detail, click here to see it.

Courtesy of Susan Clarke

2, 5, 10, 15% dolomite added to Ravenscrag Slip at cone 10R


This picture has its own page with more detail, click here to see it.

This is a buff stoneware clay. Crystal development toward a dolomite matte begins at 15%. By Kat Valenzuela.

Duplicating the G2571A dolomite matte using a Ravenscrag Slip based recipe


This picture has its own page with more detail, click here to see it.

GR10-J Ravenscrag silky matte (right) and G2571A matte (left) on a dark burning iron speckled stoneware at cone 10R. The surfaces have identical feel (the chemistries are very close). The former fires a little darker color because of the iron contributed by the Ravenscrag Slip.

Looking for a non-crazed non-cutlery marking cone 10R dolomite matte?


This picture has its own page with more detail, click here to see it.

This is G2571A cone 10R dolomite matte on an ironware body made from native North Carolina clays. Few glazes have the pleasant silky feel that this has yet are still functional. The feldspar content in the body has been tuned to establish a compromise between the warmer color that low percentages have with the higher strength that higher percentages enable. Careful porosity tests were done and recorded in an account at insight-live.com. The objective was to bring the body close to 3% absorption.

Cone 10R dolomite matte glaze with 5% manganese dioxide


This picture has its own page with more detail, click here to see it.

By Tony Hansen

A magnesia matte that breaks on contours


This picture has its own page with more detail, click here to see it.

GR10-G Silky magnesia matte cone 10R (Ravenscrag 100, Talc 10, Tin Oxide 4). This is a good example silky matte mechanism of high MgO. The Ravenscrag:Talc mix produces a good silky matte, the added tin appears to break the effect at the edges.

The power of calcined alumina to matte a magnesia glaze


Calcined alumina addition to G2934 matte

This picture has its own page with more detail, click here to see it.

This production batch of G2934 cone 6 magnesia matte glaze is firing almost glossy (upper left). Matte glaze chemistries are generally sensitive - big variations in surface character can result from small changes in firing or material chemistry/physics. This recipe relies both on high MgO and lots of Al2O3 (from high dolomite and kaolin in the recipe). A change in the frit has crossed a tipping point. But there is an amazing fix: A small addition of super fine calcined alumina (400 mesh). How small? only 1%! A small change in the frit turned it glossy so this small change has fixed it. Another factor is that greater additions of alumina (shown here are 1.5, 2.0, 2.5, and 3.0%) progressively matte it more (the slow-cool C6DHSC firing is the reason for the opacity). If the alumina was not dissolving, we would expect cutlery marking and surface staining. But neither is happening, even with additions of up to 8%, achieving stony matteness.

Inbound Photo Links



Ravenscrag Slip based dolomite matte

Two mugs with silky matte glaze
Ravenscrag Slip + 10% talc = fantastic cone 10R silky matte glaze

Two matte glazed mugs on a speckled body
Cone 10R dolomite matte effect at cone 6 oxidation


G2934 plus 10% silica actually flows more

Links

Glossary Phase Separation
Phase separation in glaze melts creates microscopic discontinuities that affect transparency, color variegation, matte surfaces, and reactive glaze effects.
Glossary Bamboo Glaze
A high temperature reduction glaze made by adding a small amount of iron oxide to a magnesia matte base glaze
Glossary Matte Glaze
Random material mixes that melt well overwhelmingly want to be glossy, creating a matte glaze that is also functional is not an easy task.
Glossary Calcination
Calcining is simply firing a ceramic material to create a powder of new physical properties. Often it is done to kill the plasticity or burn away the hydrates, carbonates, sulfates of a clay or refractory material.
Glossary Calcia Matte
Calcia matte ceramic glazes are “crystal mattes” while magnesia mattes are “microstructure mattes”. They have a smoother surface but can also have finely textured, even frosty, feathery or sugary surfaces, depending cooling and crystalliztion.
Oxides MgO - Magnesium Oxide, Magnesia
Properties Glaze Variegation
Properties Glaze Matteness
Recipes G2928C - Ravenscrag Silky Matte for Cone 6
Plainsman Cone 6 Ravenscrag Slip based glaze. It can be found among others at http://ravenscrag.com.
Recipes G2934 - Matte Glaze Base for Cone 6
A base MgO matte glaze recipe fires to a hard utilitarian surface and has very good working properties. Blend in the glossy if it is too matte.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy