0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Rate | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | LAS Body | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Interaction | Oxide Molecular Formula | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Molecular Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Reduction Speckle

A sought-after visual effect that occurs in reduction fired stoneware. Particles of iron pyrite that occur naturally in the clay melt and blossom up through the glaze

Key phrases linking here: reduction speckle - Learn more

Details

An effect created by firing a clay containing high iron mineral particles (e.g. pyrite). The iron becomes a flux in reduction and the particles melt and blossom and can even run down vertical surfaces. Plainsman Clays in Alberta, Canada, is particularly adept at making this type of body because they have raw clays that contain iron stone concretions and their grinding process can leave them large enough to blossom.

Granular additives can be added to any clay body refractory enough to host them at the intended temperature (~0.2% addition). Granular ilmenite, manganese or rutile can be used (typically 20-40 mesh size).

Specking bodies are not practical for industry because of the difficulty in maintaining a consistent fired appearance. Even slight variations in the particle size, PSD (particle size distribution), concentration, mineralogy or chemistry of the specking agent can produce noticeable differences in speckle size, color and melting and diffusing patterns. Natural speckle sources (e.g. iron stone concretions in the clay) are, by nature, inconsistent. In addition, the same reduction and temperature firing schedules time after time are essential. Packing density within the kiln, and even weather conditions, can affect the ability of the kiln to ventilate normally (to impose temperature and atmosphere). In addition, speckle bodies often contain soluble salts, which are iron-stained. While these are not obvious when a body is fired in oxidation, they will often create a glassy surface and darken fired color considerably.

Related Information

Reduction speckle: A product of iron particles in the body

And the atmosphere of the firing


This picture has its own page with more detail, click here to see it.

In reduction firing, where insufficient oxygen is present to oxidize the iron, natural iron pyrite particles in the clay convert to their metallic form and melt. The nature of the decorative speckled effect depends on the size of the particles, the distribution of sizes, their abundance, the color of the clay and the degree to which they melt and bleed at their edges. The characteristics of the glaze on the ware (e.g. degree of matteness, color, thickness of application, the way it interacts with the iron) also determine the appearance.

The same clay fired in reduction and oxidation at cone 10


This picture has its own page with more detail, click here to see it.

This is a ball clay from Manitoba. The oxidation sample has plenty of small black specks, these are an iron pyrite mineral that does not melt at cone 10 oxidation. But in the reduction firing they are being converted (reduced) to their metallic state by the lack of oxygen in the kiln. The result is vigorous melting and blossoming. Notice the surface is also glossy, this is due in part to a thin layer of iron-stained soluble salts that are melting like a glaze.

Reduction iron speckle


This picture has its own page with more detail, click here to see it.

Some of the clays mined by Plainsman Clays contain natural ironstone concretion impurities, they melt and blossom to produce speckle when fired in reduction in a gas kiln. Both of these are made from locally mined clays ground to 42 mesh. The one on the left is H550, and the one on the right is a mix containing Plainsman Fire-Red and A2 clays. The glaze is GR10-C, a magnesia matte recipe based on Ravenscrag Slip.

Here is something potters can do that industry cannot do!


This picture has its own page with more detail, click here to see it.

These mugs were fired at cone 10R. The body is L4168G5, I mixed it myself using 50% Plainsman Saint Rose Red, 40% Plainsman A2, 10% Custer feldspar. The Saint Rose clay contributes the color, the A2 the speckle and plasticity and the feldspar matures the body enough to avoid black coring. The heavy iron specking is being sourced by these very unique clays, both were ground at 42 mesh only. The left glaze is GR10-CW Ravenscrag Talc matte with added Zircopax. The right one has that same glaze on the inside and G2571A bamboo matte on the outside. The unglazed body is a beautiful deep red. These are certainly not porcelain strength but the glazes fit, the mugs are durable enough and serviceable for normal use. This type of ware is the domain of potters only, no industry would be able to babysit the touchy process it takes to make these, they would not be able to find a reliable material supply, they would not be able to maintain enough consistency and would not be able to justify to customers the high body porosity required.

Laguna B-Mix on Steroids: Wedge in some Plainsman Fire-Red!


This picture has its own page with more detail, click here to see it.

Both pieces have a transparent glaze, G1947U. The Fire-Red (a blend of Plainsman A1/M2 and St. Rose Red native clays) was slurried up, dewatered to plastic form and then wedged into the B-Mix (a commercial porcelainous whiteware body made by Laguna Clay). The left piece has 10% added Fire-Red, the other 20%, the bar in front shows the pure material). The A1 clay supplies most of the speckle, the St. Rose Red and M2 impart the color. This addition does not affect the working properties of BMix (it is highly plastic). An added benefit is that pieces dry harder and with less cracking. Fired strength and maturity are minimally affected (porosity stays around 1%). With a 20% addition, the surface of the unglazed clay is almost metallic. Silky matte glazes, like G2571A, are also stunning on a body like this.

Amazing iron-blossoms in a vitreous reduction stoneware body


Two vessels made from a vitreous metallic reduction stoneware

This picture has its own page with more detail, click here to see it.

Fire-Red is an unusual material for several reasons. It has a high iron content yet is a fireclay. It is also non-plastic. Most important, it is not ground to 200 mesh like industrial materials. These bodies demonstrate it well, left: 42.5% Fire-Red, 42.5% ball clay and 15% Custer feldspar, right: 60% Fire-Red, 30% ball clay and 10% feldspar. The ball clay adds plasticity. The feldspar gives control of the degree of vitrification (the left one has 1.3% porosity at cone 10R, the right one 1.5%). This recipe vitrifies so it does not exhibit the deep red color that Fire-Red would give if there was no feldspar. Look closely at the surface: It is covered by thousands of tiny iron-eruptions, they occurred as the iron pyrite particles liquify as FeO (because of the reduction atmosphere in the firing), and these produce a metallic appearance. And, they will bleed through an over-glaze, if present, to give stunning speckled surfaces.

Dolomite bamboo matte glazed cone 10R mug


This picture has its own page with more detail, click here to see it.

Courtesy of Susan Clarke

Heavily speckled reduction fired porcelain Shino bowl by Glenn Lewis


This picture has its own page with more detail, click here to see it.

This effect was created by wedging 10 mesh ironstone concretions into the soft porcelain.

1970s cone 10 reduction stoneware bowl by Tony Hansen


This picture has its own page with more detail, click here to see it.

Made in the mid-1970s. The body was H41G (now H441G), it had 20 mesh ironstone concretions that produced large iron blotches in reduction firing. Luke Lindoe loved to use these clays to show off the cone 10 reduction firing process that he was promoting in the 1960s and 70s. Tony was inspired by the natural rustic stoneware surfaces Luke created on both sculptural and thrown pieces, especially by how the iron speckle bled up through glazes. He made large numbers of these bowls, they showcased the clay surface on the outside and glazed designs on the inside. They proved a good testing ground for matching the thermal expansion of glaze and body (needed to produce strength and resistance to breakage).

Making your own crucibles to make your own speckle


Home made crucible

This picture has its own page with more detail, click here to see it.

I mixed a cone 6 porcelain body and a cone 6 clear glaze 50:50 and added 10% Mason 6666 black stain. The material was plastic enough to slurry, dewater and wedge like clay, dry and break into small pieces. I then melted this batch at cone 6 in a Zircopax crucible (which I make by mixing Zircopax with 3-4% Veegum, enabling throwing them on the wheel). This speckle mixture is easy to break away from the crucible because it does not completely melt and it does not stick to the zircon. I then break the black up with a special flat metal crusher we made (the shusher), size them on sieves and add them to bodies for artificial speckle. If specks fuse too much, I lower the percentage of glaze (and vice versa). Of course, the particles are glass, jagged and sharp-edged, so care is needed in handling them (a mask is essential).

Making my own home-made fired speckle for cone 6


This picture has its own page with more detail, click here to see it.

I need to control the particle size of this product. I have already smashed it up and am now sizing it. That involves getting what I can through the screen and then going at the larger-sized particles with the pestle again. This has to be done carefully, or too many fine particles are generated. I use three screen sizes in this procedure to control the distribution of particle sizes in the fired product (to more closely match reduction-fired ware). This method is also good for making your own grog, where control the distribution of sizes is important.

This can be a dusty procedure and those particles are angular and sharp and high in heavy metal, so it is best to do this outside in a breeze or with a ventilator and mask.

Emulating a speckled reduction fired stoneware in oxidation


This picture has its own page with more detail, click here to see it.

The body is Plainsman M340S. Cone 6. Left to right: G1214Z1 calciua matte base glaze with 6% titanium dioxide added. GR6-A Ravenscrag base with 10% zircopax (zircon). G2926B glossy transparent base with 10% zircon (this one produces the white "Kohler Toilet Bowl" appearance we are seeking to better). G2934Y silky magnesia matte base with 10% zircon.

Step 1 of a speckled dolomite matte at cone 6 oxidation:

This result is good enough to prove it is doable


This picture has its own page with more detail, click here to see it.

I am looking to match the reduction-fired dolomite matte mug on the right, but in cone 6 oxidation. I must duplicate the glaze color and surface character. But more difficult is the speckle size, color, density and edge bleeding. The speckle is the biggest challenge, but I met that by making my own by mixing the body and G2926B glossy glaze 50:50 and adding 10% black stain. Then I slurry it, dry it, fire it in a crucible (which I make from L4404A with an L3693E liner), crush it by hand using my shusher and screen it. I am using G2934 cone 6 magnesia matte as the glaze on this mug on the left. I add 0.5% minus 20 mesh speck to achieve this result. The next step in this project is to sieve out the smallest specks, switch to the G2934 matte glaze in the speckle recipe (the specks are too shiny here), and switch to dark brown stain instead of black. I will also need to control the degree to which the specks bleed at their edges (by adjusting the glaze:body ratio) and tune the degree of matteness (by adjusting cooling speed of the kiln). A small amount of green or blue stain is also needed to match the glaze color. There is no question that an authentic reproduction is possible; methodical testing with good records is the key to accomplishing that.

Oxidation fired speckled glaze!


M340S with white glazes

This picture has its own page with more detail, click here to see it.

The magnesia matte and calcia matte base glazes I have developed for electric firings have soft surfaces that rival the feel and utility of those achievable in reduction-fired dolomite mattes. By adding 0.2% granular manganese to M340 clay we can achieve this speckled aesthetic (outside of mug) using G2934 matte glaze.

Black coring with L4168G and L4168F


Block coring cross section

This picture has its own page with more detail, click here to see it.

These are iron reduction test bodies. The L4168G (left) is far stronger yet it has a higher percentage of Fe2O3 and much more black coring. How is that possible? Because it has 10% added feldspar. The black FeO iron is staining the feldspar black (bleeding out from each pyrite particle), helping it do its job of producing a glassy black color is not coming from the kiln atmosphere? Because the buff-burning bodies in the same kiln did not have any of this. On the right, the iron is restricted by its ability to vitrify the body by limited glass development, ending up destabilizing it instead (by increasing body thermal expansion).

Inbound Photo Links



Ravenscrag Saskatchewan clays fired at cone 10R

Links

Glossary Reduction Firing
A method of firing stoneware where the kiln air intakes and burners are set to restrict or eliminate oxygen in the kiln such that metallic oxides convert to their reduced metallic state.
Troubles Specking on Ceramic Ware
Specking, or speckling, can be both a fault or feature in fired ceramic ware - caused or produced by metal-bearing contaminants to metallic additives
Materials Iron Oxide Red
Red iron oxide is the most common colorant used in ceramic bodies and glazes. As a powder, it is available in red, yellow, black and other colors.
Minerals Iron Pyrite
Iron pyrite, or Fool's Gold, is a common metallic mineral containing about 50% iron and 33% sulfur.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy