0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Rate | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition During Ceramic Firing | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | DTA Test | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | LAS Body | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | LOI-Adjust | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Interaction | Oxide Molecular Formula | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | TGA Test | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Molecular Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Glaze Bubbles

Suspended micro-bubbles in ceramic glazes affect their transparency and depth. Sometimes they add to to aesthetics. Often not. What causes them and what to do to remove them.

Key phrases linking here: bubble-clouding, micro-bubbling, glaze bubbles, micro-bubbles, bubbling, clouding - Learn more

Details

As glazes melt, gases from the decomposition of organics, carbonates, sulphates and hydrates are generated (if the body was glazed green, or unbisqued, many more of these gases will be present). If glazes are already melting while the gases are being generated, bubbles form and are suspended in the glass melt.

For the least bubble clouding:
-Ware should be bisque-fired at the highest possible temperature (yet still be absorbent enough to glaze).
-If ware is being fired green, kilns should be soaked at the highest point possible before the glaze melts (on the way up).
-Glaze should begin melting at the highest possible temperature (because of the chemistry).
-Glaze should begin melting at the highest possible temperature (because materials sourcing the chemistry).
-Glaze ingredients should combine to have the lowest possible LOI.
-Oxide rather than carbonate colorants should be used.
-The body should generate minimal gases after the glaze has sealed.
-Glaze laydown should be as dense as possible.
-The glaze should be as thinly applied as possible.
-Glaze additives should burn out before it seals.

With increasing temperature, these bubbles will dissipate if:
-The final temperature glaze melt is fluid enough.
-The layer is thin enough.
-Surface tension of the melt is low enough to enable bubbles to merge into bigger ones that can surface.
-The kiln dwells for an adequate time when bubble surfacing occurs.

For colored, opaque and reactive glazes, less attention is necessary because the bubbles often cannot be seen. However, bubbles cloud transparents, making them appear unsightly, especially for darker colored bodies or when over underglaze colors. Strangely, at lower temperatures, it is often easier to get a crystal-clear glaze, even on red burning bodies.

Industry requires transparent glazes that can be fired quickly yet have good clarity, so considerable emphasis is placed on a bubble-free glass. Fritted glazes generate far fewer bubbles, although they can still come from the clay portion of the recipe (used for suspending the slurry), from binders, and from colored underglazes. Efforts are made to create a dense laydown to reduce air pockets in the dried glaze layer (these also produce bubbles). Highly processed bodies that use high-quality clays (low carbon) help produce a more perfect glass.

Glaze melts are not homogeneous (especially in the early stages of melting) and a beneficial side-effect of the bubbles is their mixing action. This produces a glass of less phase change (and therefore more even refraction). This is especially the case with mineral melts (e.g. Gerstley Borate).

Potters have an option many industrial users do not: Flexible firing schedules (e.g. drop-and-hold and slow-cool firing schedules).

It might seem that commercial brushing glazes for pottery should fire crystal-clear all the time, or at least better than anything you could make on your own. But this is not the case; they suffer the same problem. In their documentation and websites, manufacturers often refer to the tendency of their clear glazes to cloud if applied in too many coats (two coats are often recommended).

Related Information

Bubbles in a fritted cone 6 glaze:

What are the options?


This picture has its own page with more detail, click here to see it.

This is a cone 6 transparent fritted glaze (converted from a Gerstley Borate one). Its B2O3 content is high, sourced by Ferro Frit 3134. Bubbles in transparent glazes often plague potters; many just keep trying new glazes until one works, or give up on never finding one. Why not try to fix this problem?

Is thickness the issue? A bubble has farther to travel through a thick glaze, and the volume of bubble-generating material is greater. A glaze that clears beautifully at 0.3–0.4 mm can become a bubble bath at 0.8–1.0 mm. Often when potters find a glaze that works, they have just found one that goes on thinner and more evenly.
Is it the frit? This frit begins softening and participating in glass formation as early as 1350°F, while decomposition gases may still be arriving from clays, carbonates, the body, organics, etc. In an industrial fast-fire kiln, they need late-melters, not bubble-trappers like this. They employ fast-fire frits that melt later. That being said, potters do have flexible firing, so this could still be made to work by slowing down the firing leading up to 1350. It also could be held at top temp, then either slow-cooled or a drop-and-hold.
Is it the recipe? Notice the big bubbles; they started as little ones that merged. Given enough time, big ones break at the surface, but only under the right conditions: Low enough melt viscosity and surface tension. Strangely, some old recipes sourcing high boron from Gerstley Borate had surprisingly few problems with bubbles! Why? While GB has substantial LOI itself, it appears that it can be its own fining agent with the right viscosity-versus-temperature curve. Its boron enters the melt later, and the melt develops unevenly, and may create localized channels and variable viscosity zones for easier bubble escape. The larger bubbles may better move laterally by combinations of lower surface tension, layer thickness and temperature gradients, and downward movement that creates shear.
Is it the melt surface tension?

Let's assume this glaze melt has high surface tension. It pulls liquid inward around each bubble, stabilizing them round and making rupture more difficult. But if surface tension drops, even slightly, bubbles deform more easily and adjacent ones merge. What could help? Industrial technicians have found that surprisingly small recipe changes can really help with bubble release.

Glaze bubbles on buff and red burning bodies at cone 6


This picture has its own page with more detail, click here to see it.

These Plainsman Midstone and Redstone cups are fired to cone 6 with M340 Transparent glaze liner (these are raw materials that body manufacturers incorporate into their products in fairly high percentages). Notice how many more glaze bubbles there are with the red cup. This is typical using other transparent glazes also. To get a bubble-free clear on this red burning body a glaze having a higher melt fluidity, lower melt viscosity, later melting and a fining agent is needed. And we found two: GA6-B and G3806C.

A light bulb moment in solving bubble clouding:

The same black engobe with two transparent glazes.


A bubble clouding transparent glaze

This picture has its own page with more detail, click here to see it.

This is a buff stoneware body, Plainsman M340. A L3954F black engobe was applied inside and upper-outside at leather hard. The piece was fired at cone 6 using the PLC6DS schedule. The inside, totally clouded glaze, is G2926B. Outside is GA6-B Alberta Slip amber transparent. This inside glaze is crystal-clear on other bodies (and on this one without the black engobe). The black stain in the engobe appears to be the issue. How?

Underglazes (or engobes) become a semi-dense layer and impede LOI by slowing gas diffusion. If the glaze then melts early and lacks viscosity, remaining channels of escape are sealed (increasing bubbling dramatically). Double-melt interfaces can form between vitreous engobes and glaze when the former softens, the clear glaze begins melting. Gases get trapped at the boundary, being generated at the exact wrong time during the firing.

Look at the outside amber transparent glaze, GA6-B. Although also early melting and on the same engobe, it has very little micro-bubble clouding! Why? It contains a lot of Alberta Slip, a material that is not finely ground like others. Particles across the range from 60-200 mesh are present; these are likely acting as a fining agent that enables bubble merging. The larger bubbles break at the surface because of sufficient melt mobility and lower melt surface tension.

Underglazes require a fluid melt transparent

But extra melt fluidity comes at a cost


A fluid melt glaze over underglaze

This picture has its own page with more detail, click here to see it.

These porcelain mugs were decorated with the same Amaco Velvet underglazes (applied at leather hard), then bisque fired, dipped in clear glaze and fired to cone 6 (using a drop-and-hold schedule). While the G2926B clear glaze (left, A) is a good glossy transparent for general use, its melt fluidity is not enough to clear the LOI micro-bubble clouds that dull the colors below (strangely, underglaze colors can generate them too). However, the G3806C recipe (right, B) has a more fluid melt, which is one factor that better enables bubble escape. Its melt also has a lower surface tension. An additional factor is thickness. A thinner layer of B would be even better (brushing glazes enable thin layering).

But B has downsides. Running is one, but not a factor here because we want it thin. Its high flux content also means it fires less durable. And, its high KNaO content raises the thermal expansion (COE) and thus the danger of crazing. Although it fits this porcelain, it crazes on others.

Four boron frits with vastly different melting:

Knowing about this could debubble your clear glaze.


This picture has its own page with more detail, click here to see it.

Industry, late-melting glazes are a must for fast fire because there is no time for glazes to debubble. The later they melt (while still melting well at the target temperature), the more LOI gases of decomposition (generated by the body, glaze materials, glaze & body additives) can be expelled first. What about potters? These melt flow tests are of specific interest to anyone making clear glazes using frit 3134. They compare four common Ferro products fired to 1750F: Frit 3249 (29% B2O3), frit 3124 (14% B2O3), frit 3195 (23% B2O3) and frit 3134 (23% B2O3). Surprisingly, the one having the most B2O3 starts melting the latest (more than 200F after 3134), this is because of the amount of MgO in the formula. So, if your transparent glaze contains any MgO (G2926S, for example, contains 0.15 molar), the more that can be supplied using this (instead of 3134), the later the glaze will melt. Likewise, frit 3124 is a better choice than 3134 in cases where the percentage of clay can be reduced (since it supplies much more Al2O3). Glazes containing high percentages of feldspar are least likely to benefit because the main alternative source of KNaO is frit 3110, and it melts even sooner than 3134 (an exception is cases where the glaze also has high MgO and B2O3).

Same glaze chemistry, very different LOIs.

Look at the bubbles!


This picture has its own page with more detail, click here to see it.

These two GBMF test balls were melted on refractory tiles to compare their melting behaviour. Their calculated oxide chemistries are almost identical, but their recipes are very different. G2931F (left) contains 29% Ulexite, driving its calculated LOI to 14.3%. G2931K (right) sources its boron from frits, reducing the LOI to just 3.1%. The difference is striking! The high-LOI glaze is full of large bubbles that were unable to escape or clear before the melt stiffened during cooling. Although ulexite releases most of its chemically bound water before significant glaze melting, that early gas evolution can contribute to foaming and trapped bubbles as melting progresses. The fritted glaze is much clearer, although it still contains fine bubbles. These may be associated with the kaolin or other sources of entrained gas.

The GBMF test exaggerates gas-retention behaviour, which is precisely why it is useful for comparing recipes, but it does not necessarily predict the appearance of a thin glaze layer on ware.

Bubble city with Seattle Midnight body:

With G3806C glaze at cone 01, 4 and 5


This picture has its own page with more detail, click here to see it.

This black body is made by Seattle Pottery Supply. Surfaces like this are obviously not functional, but for decorative ware? Yes! How does this happen? This body contains a material that is adding to its LOI (likely raw or burnt umber). Not just that, but the gases are being expelled at the wrong time. How is that? The glaze is fluid at cone 6 and begins melting way down around cone 04. It melts long before the gases of decomposition from the body are finished being expelled. So they have to bubble up through the glaze, creating the effect you see here. This body is actually over-mature and brittle at cone 5, but at cone 01 its strength is fairly good.

Zircopax as a fining agent to de-bubble a stained glaze


This picture has its own page with more detail, click here to see it.

The cone 03 porcelain cup on the left has 10% Cerdec encapsulated stain 239416 in the G2931K clear base (this is not an underglaze with a transparent over it). The surface is badly orange-peeled because the glass is full of micro-bubbles that developed during the firing. Notice that the insides of the cups are crystal-clear, no bubbles. So here, they are a direct product of the presence of the stain. The glaze on the right has even more stain, 15%. Why isn't it even worse? It also has a 3% addition of Zircopax (zircon), which acts as a fining agent. As you can see, this makes a dramatic difference. Suppliers of encapsulated stains even recommend a zircon addition, but are often unclear about why. This is the reason.

The yellow on the right could be improved further with a slow-cool or drop-and-hold firing. And if the glaze was reformulated to use a later melting frit (so fewer bubbles even get trapped).

Glaze with an encapsulated stain is bubbling. It needs Zircopax.


Glaze orange peel defect

This picture has its own page with more detail, click here to see it.

These two pieces are fired at cone 6. The base transparent glaze is the same - G2926B Plainsman transparent. The amount of encapsulated red stain is the same (11% Mason 6021 Dark Red). But two things are different. Number 1: 2% Zircopax (zircon) has been added to the upper glaze. The stain manufacturers recommend this, saying that it makes for a brighter color. However, that is not what we see here. What we do see is the particles of unmelting zircon acting as seeds and collection points for the bubbles (the larger ones produced are escaping). Number 2: The firing schedule. The top one has been fired to approach cone 6 and 100F/hr, held for five minutes at 2200F (cone 6 as verified in our kiln by cones), dropped quickly to 2100F and held for 30 minutes.

LOI horse race with a surprising winner and loser


A chart showing weight-loss vs firing temperature for common ceramic materials

This picture has its own page with more detail, click here to see it.

This chart compares the decompositional off-gassing (% weight Loss on Ignition) behavior of six glaze materials (there are many more). Each was heated through the range 500-1700F at 350F/hr. It is amazing how much weight some can lose on firing. For example, 100 grams of calcium carbonate generates 44 grams of CO2! Magnesium carbonate even more. But the main message of this chart is that some late gassers overlap early melters. That can be a problem (causing glaze bubbles, blisters, pinholes). The talc in this test is an example: It did not finish gassing until 1650F. Yet many fritted and Gerstley Borate glazes have already begun melting by then.

There are two takeaways here. The biggest weight loser is not the biggest troublemaker. What matters is how gas release overlaps glaze sealing. Calcium carbonate illustrates this; its high carbonate content can still produce a clear glaze (when gases can clear ahead of any melting). And the talc, although having a small LOI, is a potential troublemaker when the glaze melt cannot effectively clear the bubbles.

Calcium carbonate and glaze bubbles


This picture has its own page with more detail, click here to see it.

The two cone 04 glazes on the right have the same chemistry but the center one sources it's CaO from 12% calcium carbonate and ulexite (the other from Gerstley Borate). The glaze on the far left? It is almost bubble free yet it has 27% calcium carbonate. Why? It is fired to cone 6. At lower temperatures carbonates and hydrates (in body and glaze) are more likely to form gas bubbles because that is where they are decomposing (into the oxides that stay around and build the glass and the ones that are escaping as a gas). By cone 6 the bubbles have had lots of time to clear.

Close-up of cone 10R celadon bubbles suspended in the glass


This picture has its own page with more detail, click here to see it.

This is happening because this glaze lacks flux and is not fluid enough to enable their migration. In the upper half they are more evident (double thickness).

A body containing manganese bubbles the glaze


This picture has its own page with more detail, click here to see it.

Laguna Barnard Slip substitute fired at cone 03 with a Ferro Frit 3195 clear glaze. The very high bubble content is likely because they are adding manganese dioxide to match the MnO in the chemistry of Barnard (it gases alot during firing).

Is clear glazing a dark burning oxidation stoneware a good idea? Likely not.


Clear glaze bubble clouding

This picture has its own page with more detail, click here to see it.

Dark bodies tend to have more carbon impurities and the burnout of these can generate gases that create bubbles in the glaze. Because of the dark background, the bubbles impart a muddy look. The body on the left is a finer particle size, so the lower thinner glazed section is a partial success, but the upper section is bubbling. The body on the right, although a more pleasant red color, is bubbling worse. Notice also that the warm color of the body is at least largely lost under the glaze. At its worst pinholes can appear.

Perfect storm to create massive bubbling in a low fire kiln


This picture has its own page with more detail, click here to see it.

The clay is terra cotta. It is volatile between 04 and 02, becoming dramatically more dense and darker colored. The electronic controller was set for cone 03, but it has fired flat (right-most cone), that means the kiln went to 02 or higher. At 02 the body has around 1% porosity, pushing into the range where the terra cotta begins to decompose (which means lots of gas expulsion). The outsides of some pieces blistered badly while the insides were perfect (because they got the extra radiant heat). The firing was slow, seven hours. Too long, better to make sure ware is dry and fire fast. Another problem: The potter was in a rush and the pieces were not dry. These factors taken together spelled disaster.

2% iron oxide in a glossy terra cotta glaze gives better color, less clouding


Two brilliantly transparent glazed terra cotta mugs

This picture has its own page with more detail, click here to see it.

Both pieces are the same clay body, Plansman L215. Both are fired to cone 03. Both are glazed using G1916Q borosilicate recipe. The glaze on the piece on the left has 2% added iron oxide (sieved to 80 mesh). Each particle or agglomerate of iron (which is refractory in this situation) acts to congregate the micro-bubbles so they can better exit the glaze layer. Notice also how much richer the color is as a result. The piece on the right, without the added iron oxide, is neither as red nor as transparent. Of course, I had to be careful not to apply the glaze too thickly on both.

Micro bubbles in low fire glaze. Why?


This picture has its own page with more detail, click here to see it.

Left: G1916Q transparent fired at cone 03 over a black engobe (L3685T plus stain) and a kaolin-based low fire stoneware (L3685T). The micro-bubbles are proliferating when the glaze is too thick. Right: A commercial low fire transparent (two coats lower and 3 coats upper). A crystal clear glaze result is needed and it appears that the body is generating gases that cause this problem. Likely the kaolin is the guilty material, the recipe contains almost 50%. Kaolin has a 12% LOI. To cut this LOI it will be necessary to replace some or all of the kaolin with a low carbon ball clay. This will mean a loss in whiteness. Another solution would be diluting the kaolin with feldspar and adding more bentonite to make up for lost plasticity.

Why is this transparent so full of bubbles?


This picture has its own page with more detail, click here to see it.

An example of how a micro-bubble population in the matrix of a transparent glaze can partially opacify it. If this glaze was completely transparent, the red clay body would show much better. However this is not the fault of the glaze. On a white body it would be more transparent. The problem is the terra cotta body. This is fired at cone 02. As the body approaches vitrification the decomposition of particles within it generate gases that bubble up in to the glaze. A positive aspect of this phenomena that this glaze could be opacified using a lower percentage of zircon.

This type of glaze responds better to opacifier additions.

Example of how bubbles dissipate in a glaze with increasing temperature


This picture has its own page with more detail, click here to see it.

This is a 45% Gerstley Borate recipe melted in crucibles at increasing temperatures. Although the recipe is well melted at cone 2, it is still not fluid enough to enable their migration in the time available. By contrast, the melt at the upper temperature is much less viscous, enabling all bubbles to completely clear on the thinner sections. If this glaze were applied to ware it would be in a thin layer and the bubbles would likely clear at cone 6. Not to be ignored is the degree to which the thousands of bubbles passing upward through the melt have helped to mix the melt and remove discontinuities in the cone 7 and 8 specimens.

What material makes the tiny bubbles? The big bubbles?


This picture has its own page with more detail, click here to see it.

These are two 10 gram GBMF test balls of Worthington Clear glaze fired at cone 03 on terra cotta tiles (55 Gerstley Borate, 30 kaolin, 20 silica). On the left it contains raw kaolin, on the right calcined kaolin. The clouds of finer bubbles (on the left) are gone from the glaze on the right. That means the kaolin is generating them and the Gerstley Borate the larger bubbles. These are a bane of the terra cotta process. One secret of getting more transparent glazes is to fire to temperature and soak only long enough to even out the temperature, then drop 100F and soak there (I hold it half an hour).

Glaze bubbles behaving badly!

We see it in a melt fluidity test.


This picture has its own page with more detail, click here to see it.

These melted-down-ten-gram GBMF test balls of glaze demonstrate the different ways in which tiny bubbles disrupt transparent glazes. These bubbles are generated during firing as particles in the body and glaze decompose. This test is a good way to compare bubble sizes and populations, they are a product of melt viscosity and surface tension. The glaze on the top left is the clearest but has the largest bubbles, these are the type that are most likely to leave surface defects (you can see dimples). At the same time its lack of micro-bubbles will make it the most transparent in thinner layers. The one on the bottom right has so many tiny bubbles that it has turned white. Even though it is not flowing as much it will have less surface defects. The one on the top right has both large bubbles and tinier ones but no clouds of micro-bubbles.

Cone 6 glazes can seal the surface surprisingly early - melt flow balls reveal it


This picture has its own page with more detail, click here to see it.

These are 10 gram balls of four different common cone 6 clear glazes fired to 1800F (bisque temperature). How dense are they? I measured the porosity (by weighing, soaking, weighing again): G2934 cone 6 matte - 21%. G2926B cone 6 glossy - 0%. G2916F cone 6 glossy - 8%. G1215U cone 6 low expansion glossy - 2%. The implications: G2926B is already sealing the surface at 1800F. If the gases of decomposing organics in the body have not been fully expelled, how are they going to get through it? Pressure will build and as soon as the glaze is fluid enough, they will enter it en masse. Or, they will concentrate at discontinuities and defects in the surface and create pinholes and blisters. Clearly, ware needs to be bisque fired higher than 1800F.

Has a cone 5 bisque released Pandora particles?


Bubbles and blister in a low fire ceramic tile

This picture has its own page with more detail, click here to see it.

An art tile company is bisque firing a heavily grogged red stoneware body to cone 5 and then finishing with a range of low temperature boron glazes. But these glaze bubble and blister defects are happening! There appears to be some sort of LOI gas-monster particles present. They could be in the grog. And, the body contains two dark burning fireclays, both could contain also rogue particles. To identify them a sieve could be used to pull out the larger ones (e.g. 35 or 42 mesh) and these could be spread in a thin layer onto a porcelain tile and fired to cone 5. Taking closeup photos before and after should spot the guilty ones, they will have a visibly different form (e.g. melting, puffing up, altered color). These pandora particles seem to be activated at cone 5 and capable of continuing to gas even at low refire.

What does it take to get a crystal-clear low fire transparent? A lot!


This picture has its own page with more detail, click here to see it.

These three cups are glazed with G1916S at cone 03. The glaze is the most crystal clear achieved so far because it contains almost no gas producing materials (not even raw kaolin). It contains Ferro frits 3195 and 3110 plus 11 calcined kaolin and 3 VeeGum. Left is a low fire stoneware (L3685T), center is Plainsman L212 and right a vitreous terra cotta (L3724F). It is almost crystal clear, it has few bubbles compared to the kaolin-suspended version. These all survived a 300F/icewater IWCT test without crazing!

An ultra-clear brilliantly-glossy cone 6 clear base glaze? Yes!


This picture has its own page with more detail, click here to see it.

I am comparing 6 well known cone 6 fluid melt base glazes and have found some surprising things. The top row are 10 gram GBMF test balls of each melted down onto a tile to demonstrate melt fluidity and bubble populations. Second, third, fourth rows show them on porcelain, buff, brown stonewares. The first column is a typical cone 6 boron-fluxed clear. The others add strontium, lithium and zinc or super-size the boron. They have more glassy smooth surfaces, less bubbles and would should give brilliant colors and reactive visual effects. The cost? They settle, crack, dust, gel, run during firing, craze or risk leaching. Out of this work came the G3806E and G3806F.

Two glazes with the same chemistry but different melt flows

Hint: It is the LOI difference


This picture has its own page with more detail, click here to see it.

At low temperatures, potters want transparents with good clarity to support brilliant colors. Especially on terra cotta bodies. A melt flow test like this enables a comparison one cannot do on using glazed test tiles.

These are two low-temperature glazes being compared on a GLFL test: G2931F and G2931K. They have the same chemistry. But F gets its boron from Ulexite, a material with a high LOI (notice how the escaping and bubbling gases of its decomposition have disrupted the downward flow). The frit-sourced boron version on the right flows cleanly and contains almost no obvious bubbles.

Does this mean that the G2931F version is useless? Not exactly. LOI gases can often escape well from a thin glaze layer. I used the K version successfully on many pieces. In a thin layer, the ulexite seems to act as its own fining agent, like Gerstley Borate, and the bubbles do merge clear well enough.

Adding iron to a clear glaze has cleared the micro-bubbles!


This picture has its own page with more detail, click here to see it.

The glaze on the right is a transparent, G2926B, on a dark burning cone 6 body (Plainsman M390). On the left is the same glaze, but with 4% red iron oxide added. The entrained microbubbles are gone and the color is deep and much richer. It is not clear how this happens, but it is some sort of "fining" and is certainly beneficial. In other circumstances, we have seen big benefits with only 2% iron added.

Inbound Photo Links



Comparing two brands of calcium carbonate


Bubbles in Terra Cotta transparent glazes. What to do?


Red burning clays bubble glazes more


Reduction and oxidation porcelains


Frits melting before carbon expulsion

One glaze is transparent, the other milky because it is filled with micro bubbles.
Iron oxide as a fining agent to debubble a low fire transparent

Terra cotta mugs with cloudy glazes
Clouding varies with these cone 04 terra cotta glaze recipes

Links

Glossary Carbon trap glazes
A type of ceramc glaze.
Glossary LOI
Loss on Ignition is a number that appears on data sheets test results of ceramic materials and bodies. It refers to the amount of weight lost as it decomposes to release water vapor and various gases during firing.
Glossary Glaze Blisters
Blistering is a common surface defect that occurs with ceramic glazes. The problem emerges from the kiln and can occur erratically in production. And be difficult to solve.
Glossary Surface Tension
In ceramics, surface tension is discussed in two contexts: The glaze melt and the glaze suspension. In both, the quality of the glaze surface is impacted.
Glossary Transparent Glazes
Every glossy ceramic glaze is actually a base transparent with added opacifiers and colorants. So understand how to make a good transparent, then build other glazes on it.
Glossary Drop-and-Soak Firing
A kiln firing schedule where temperature is eased to the top, then dropped quickly and held at a temperature 100-200F lower.
Glossary Ceramic Glaze Defects
Ceramic glaze defects include things like pinholes, blisters, crazing, shivering, leaching, crawling, cutlery marking, clouding and color problems.
Glossary Fining Agent
Individual tiny bubbles in a glaze melt can coalesce around the undissolved particles of a fining agent, the growing bubble swallowing others around it and finally exiting at the surface.
Tests Glaze Melt Fluidity - Ball Test
A test where a 10-gram ball of dried glaze is fired on a porcelain tile to study its melt flow, surface character, bubble retention and surface tension.
Firing Schedules Cone 6 Drop-and-Soak Firing Schedule
350F/hr to 2100F, 108/hr to 2200, hold 10 minutes, freefall to 2100, hold 30 minutes, free fall

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy