0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Rate | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition During Ceramic Firing | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | DTA Test | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | LAS Body | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | LOI-Adjust | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Interaction | Oxide Molecular Formula | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | TGA Test | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Molecular Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Celadon Glaze

A type of stoneware glaze normally fired in a high temperature reduction atmosphere kiln. It is transparent and stained green or blue by the presence of iron oxide.

Key phrases linking here: celadon glaze - Learn more

Details

A green or blue-green reduction fired glaze that has been stained using iron oxide. Celadons were first developed by the ancient Chinese. The celadons that potters are accustomed to firing today are glossy transparent whereas the ancient versions were more waxy and opaque. Thus there is dispute among practitioners and purists about what exactly a celadon really should be or what glaze can truly be labelled 'Celadons'. There are many books and webpages on the subject.

Typically celadon glazes are employed on porcelain but can also be used effectively on stonewares. Modern Celadons usually possess their high gloss because of high amounts of sodium and potassium, these oxides also cause the crazing often seen. However this problem can be solved by substituting some of the Na2O with lower expansion MgO or CaO and increasing the SiO2 (using glaze chemistry of course). Celadons have traditionally been fired at cone 10 but lower temperatures are possible with the addition of more flux (e.g. Gerstley Borate).

Blue celadons typically have high sodium/potassium, high silica, not too much iron, and low titanium (Grolleg kaolin is a good option to minimize the TiO2). Some claim that a little tin oxide and/or barium carbonate will help with the blue color. Some people are investigating creating celadons for cone 6 oxidation using stains to impart the color.

Related Information

Example of a logo done using a polymer plate


A mug with an embosses logo make by a letterpress stamp

This picture has its own page with more detail, click here to see it.

The buff stoneware mug is fired at cone 10R and celadon glazed. The recesses were colored with a tenmoku glaze (on bisque by painting it into the recesses and sponging away the high spots). An outer containment line on the plate prevented the outside line from smearing outward and it provided a definite profile for cut-out after stamping.

Start glaze chemistry by learning when you don't need it!

A high feldspar glaze is a good example


A runny, amber, crazed glaze

This picture has its own page with more detail, click here to see it.

This reduction celadon is crazing badly. Why? Its chemistry is dominated by feldspar, which supplies lots of K2O and Na2O fluxes. Scores of recipes being traded online contain 50% or more feldspar; they benefit from these powerful fluxes but inherit their high thermal expansion (COE). Many work only because the body happens to have sufficiently high expansion - often aided by significant residual quartz.

Crazing is more than a cosmetic problem in functional pieces. It reduces ware strength and durability, can compromise food safety and turn into a customer complaint. Let's fix it, starting without chemistry:

Close-up of cone 10R celadon bubbles suspended in the glass


This picture has its own page with more detail, click here to see it.

This is happening because this glaze lacks flux and is not fluid enough to enable their migration. In the upper half they are more evident (double thickness).

GR10-E Ravenscrag:Alberta Slip with 10% calcium carbonate


This picture has its own page with more detail, click here to see it.

At cone 10R this produces an overly melted glaze. It also crazes.

Ravenscrag GR10-E celadon glaze


This picture has its own page with more detail, click here to see it.

(50:50 Ravenscrag Slip:Alberta Slip) at cone 10R on porcelain (right) and stoneware (left).

GR10-E 50:50 Alberta Slip:Ravenscrag Slip celadon at cone 10R


This picture has its own page with more detail, click here to see it.

On a white stoneware and a porcelain. The glaze is transparent, it has depth and varies in shade according to thickness, breaking to a much lighter shade on the edges of contours.


This picture has its own page with more detail, click here to see it.

50:50 Alberta Slip:Ravenscrag Slip cone 10R celadon on iron stoneware, buff stone and porcelain.

Just enough iron in this celadon to highlight the design


This picture has its own page with more detail, click here to see it.

There is only 0.35% iron oxide in this recipe, as much as ten time less than normal. But this is just enough to provide a darker shadow (where the glaze is thicker) at the edges of the design. This is porcelain fired at cone 10 reduction by Janel Jacobson.

Iron oxide additions to a transparent glaze:

In reduction firing, iron is amazing


Glazes range from celadon to heavy iron crystal surface

This picture has its own page with more detail, click here to see it.

Iron oxide is an amazing glaze addition in reduction. Here, I have added it to the G1947U transparent base. It produces:

These samples were cooled naturally in a large reduction kiln using the C10RPL firing schedule; the crystallization mechanism would be heavier if it were cooled more slowly (or less if cooled faster). The 7% one in this lineup is quite interesting; a minimal percentage of cobalt-free black stain could likely be added to create an inexpensive and potentially non-leaching jet-black glossy.

Alberta Ravenscrag Cone 6 Brilliant Celadon


This picture has its own page with more detail, click here to see it.

The magic of this recipe is the 5% extra frit, that makes the melt more fluid and brilliant and gives the glaze more transparency where it is thinner on edges and contours. The extra iron in the Plainsman P380 (right) intensifies the green glaze color (vs. Polar Ice on the left).

The specks are cobalt oxide agglomerates that were made by slurrying cobalt oxide and bentonite, then crushing it to sizes large enough to make the specks.

Inbound Photo Links



Ravenscrag Alberta Slip Celadon mug by Tony Hansen

Links

URLs http://en.wikipedia.org/wiki/Celadon
Celadon on Wikipedia
Glossary Ceramic Glaze
Ceramic glazes are glasses that have been adjusted to work on and with the clay body they are applied to.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy