0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Rate | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition During Ceramic Firing | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | DTA Test | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | LAS Body | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | LOI-Adjust | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Interaction | Oxide Molecular Formula | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | TGA Test | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Molecular Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Specific gravity

In ceramics, the specific gravity of slurries tells us their water-to-solids ratio. That ratio is a key indicator of performance and enabler of consistency.

Key phrases linking here: specific gravity, solids loading, high-solids, low-solids - Learn more

Details

The specific gravity of a liquid suspension is a comparison of its weight with the weight of an equal volume of water. Water has a specific gravity of 1.0, or 1 gram per cc. A slurry with a specific gravity of 1.8 is thus 1.8 times heavier than water. The specific gravity of ceramic slurries rises as the percentage water content drops. Through deflocculation, the specific gravity of a slurry can be increased while maintaining fluid flow. In ceramics, the term "solids loading" is often used, and specific gravity is the measure of it. Thus, high-solids slurries have less water; low-solids slurries have more water. Engobe, underglaze and glaze slurries must be monitored for this.

Measuring Specific Gravity:

Specific gravity is very important in the production of casting slips where low-as-possible (or, more accurately, low-as-practical) water content is needed. Hobbyists and potters typically target around 1.75, whereas in industry 1.8 or higher is needed (especially in sanitaryware). Achieving a slurry having a specific gravity approaching twice that of water is only possible using the deflocculation process. Some slurries need to be both high-solids and low viscosity (e.g. for quick dipping of ware). When slurries are not behaving normally (e.g. settling, gelling, casting too slowly or unevenly, not draining from the mold properly, not releasing, producing a powdery surface), the first step in isolating the reason is a specific gravity measurement for comparison with historical measurements. Corrections in water content are always made before assessing whether the amount of deflocculant is correct. A good example of the logic is a slurry having too low a specific gravity: It can exhibit similar casting issues to an over-deflocculated one; the best way to know whether a water or deflocculant change is needed is knowing the specific gravity.

Glazes do not have a universally desirable specific gravity range like casting slips. The same glaze can be used effectively by different people and in different processes, having quite different specific gravities. We have seen production glazes with specific gravities approaching 1.8. Some industries even prepare their glazes up to 2.0 (obviously highly deflocculated), something that would be impossible for the average potter. Commercial brushing glazes (for use by hobbyists and potters) can have specific gravities ranging from below 1.25 up to 1.55 (some companies emphasize brushability and their products are on the lower end). Instructions for dipping glaze products can vary from recommending 1.4 SG (for a 5-second dipping time) to 1.5 (for a 1-second time). Caution is needed here. Some glaze recipes, when mixed to the apparent correct viscosity (having no additives), will have a fairly high specific gravity (e.g. 1.55-1.6). These commonly settle out into a hard layer on the bottom of the container. Raising the water content (thus lowering the specific gravity) and gelling the slurry (using vinegar for example) is a way to deal with this. Notwithstanding this, doing the opposite, deflocculating the slurry, is also a way to prevent sedimentation (provided it is still viscous). Potters who make their own glaze generally do best with them in the 1.45 range.

Dipping glaze slurries that are 'gelled' work best for potters because they apply more evenly, drip less and do not settle. To be gelled, the specific gravity has to be lower than normal, and then a flocculant is added to bring it back to a creamy consistency. For many common partially-fritted glaze recipes, this occurs around 1.43-1.45 specific gravity. The addition of Epsom salts or vinegar to the slurry gels it and imparts the property of thixotropy. The important thing is to determine, by experience with a specific glaze, what specific gravity and flocculation procedure works well, then stick to that for future batches.

Dark-colored, paint-on glazes used for detail work need to have a high specific gravity so they can cover well with a single brush stroke (e.g. 1.55). Clear glazes that need to be applied (by painting) in a thin layer need a lower specific gravity (e.g. 1.25).

It may be that measuring the water content is easier and more appropriate for what you are doing. It can also be easier to measure if you have an automated device or a heat lamp.

Brushing Glazes

Specific gravity indicates how much solid is being carried in relation to the water, but it does not describe how the slurry flows. Two products having the same specific gravity can behave very differently because of differences in particle size, particle shape, surface area, clay content, stain type, soluble salts, dispersion and gum content.

A higher specific gravity generally deposits more ceramic powder in each coat while introducing less water into the ware. This can enable a thicker layer with fewer coats and reduce drying shrinkage. It is particularly valuable when decorating unfired ware, where excess water can soften or slake the surface.

However, increasing specific gravity too far can cause brush drag, poor levelling, cracking, screen blockage or difficulty mixing the product. Adding gum simply to make a dilute slurry appear thick does not compensate for inadequate solids loading. Such a mixture may look creamy yet deposit very little ceramic material and shrink excessively during drying.

Related Information

Slip having proper rheology is so much better


This picture has its own page with more detail, click here to see it.

This deflocculated slurry of 1.79 specific gravity (only 28% water) has just been poured into a mold. The mold is dry, the wall thickness of the bowl will build quickly and the liquid level will sink only slightly. It can be drained in minutes (for a wall thickness of 3-4 mm). The clay is not too plastic (too fine particle sized) so it is permeable enough to enable efficient water migration to the plastic face. If the specific gravity of this slip was too low (too high a percentage of water) the liquid level would sink drastically during the time in the mold, take longer to build up a wall thickness and water-log the mold quickly. If the slip contained too much deflocculant it would cast slower, settle out, form a skin and drain poorly. If it had too little deflocculant it would gel in the mold and be difficult to pour out. The rheology is just right.

When to use a hydrometer and when not to


This picture has its own page with more detail, click here to see it.

If a glaze has already been mixed and gelled to give it thixotropy these things won't bob up and down to home in on the right level. If the glaze is watery enough there are other issues. The one on the right has a 1.0-1.7 scale. Since most pottery glazes need to be 1.4-1.5 specific gravity (40-50 on this scale) it is difficult to get a very accurate reading. And it is long, you will need a container tall enough to float it and enough glaze to fill it. The small hydrometer appears better, it has a scale of 1.2 to 1.45. But it really bobs up and down (so it is even more important that the slurry be runny and thin to give it the freedom to do so). But glaze slurries are creamy. So it is better to weigh a measured volume of glaze slurry and calculate the SG instead. The easiest is a 100cc graduated cylinder (from Amazon.com), if 100 ccs weighs 140 grams, that is 1.4 specific gravity. You don't even have to pour in 100cc, just pour in any amount and divide the weight by the amount.

More problems measuring glaze specific gravity using a hydrometer


This picture has its own page with more detail, click here to see it.

Potters sometimes call this a "floating thingy". Maybe, because of the problems it presents, it does not make a big enough impression to remember the name! Because of the length of the hydrometer the only container we have is this graduated cylinder. I have to fill it just the right level so it reads near the top. OK, fine. But the hydrometer needs to bob up and down to find home. However, this glaze has our desired thixotropy, which prevents free movement. OK, I will carefully help it find home by pushing it down a little. But then it doesn’t want to bob back up! Ok, I’ll pull it up ... then is doesn't want to go back down to where it should float. Not great. Next problem: The glaze is opaque, I can’t see the reading. Yikes! A better way would be to throw out the hydrometer and just tare the empty cylinder on a scale, fill it to 100 and read the SG as the weight/100. Or fill it to any mark and divide the weight by that.

Are cheap plastic graduated cylinders useful?

Yes, you can calibrate them yourself.


This picture has its own page with more detail, click here to see it.

Graduated cylinders like this are inexpensive (e.g. Amazon.com). Of course, these cheap plastic ones are not accurate. But, there is one factor that makes them useful: They are light and can thus be used to measure specific gravity on a 200g scale. There is a way to make these accurate enough for a potter: Calibrate them by checking with 100g and 50g of water, just mark the levels using a Sharpie.

Measure specific gravity using a scale and measuring cup


This picture has its own page with more detail, click here to see it.

The specific gravity of a suspension is simply its weight compared to water (water weighs 1g per cc). For example, different glazes optimize to different specific gravities (e.g. 1.45 is typical for stoneware glazes). Casting slips typically have specific gravities of 1.75-1.8. This plastic measuring cup accommodates 500g. I have already counter-weighed it on our 0.1g scale and filled it with 500 grams of water to verify the accuracy of the 500g marking (mark the correct level with a felt pen or sticker if needed). Now, I am filling the cup with the slurry to the same level. The specific gravity will be that weight divided by 500.

Specific gravity using a scale and graduated cylinder:

It doesn't matter how high you fill it


Slurry in graduated cylinder

This picture has its own page with more detail, click here to see it.

In this case, I just need an approximate measure. So I counterbalance a graduated cylinder on a 0.01g scale and pour in some slurry. Fill it to any level that does not exceed the weight the scale can handle. Divide the weight by the volume. In this case, it weighs 60.6g and the volume is 41. That calculates to about 1.47 specific gravity. The higher it is filled, the higher the quality of the graduated cylinder and the better you are at reading the level, the more accurate the measurement will be. After adding more water to this glaze, I will measure again, filling it to near the 100cc level. I have to use a plastic cylinder because our glass one is too heavy for this scale to handle (its max is 200g).

A casting slip of 1.9 specific gravity. Should we use it?


This picture has its own page with more detail, click here to see it.

A hydrometer is being used to check the specific gravity of a ceramic casting slip in a graduated cylinder. Common traditional clay-containing ceramic slips are usually maintained around 1.75-1.8. In this case the slurry was too heavy, almost 1.9. Yet it is very fluid, why is this? It has both too much clay and too much deflocculant. While it is possible to use such a slip, it will not drain as well and it will gel too quickly as it stands. It is better to settle for a lower specific gravity (where you can control the thixotropy and it is easier to use). It might have been better to simply fill a 100cc cylinder and weigh it to get the specific gravity (slurries that are very viscous do not permit hydrometers to float freely).

What to do when glazes drain and drip like this


Two mugs, one with glaze drips

This picture has its own page with more detail, click here to see it.

These are the same dipping glaze, it is variegated, and drips look ugly on fired ware. The slurry of the one on the left had a specific gravity of 1.45, it was creamy and appeared to be good. However, when this bisque porcelain mug was pulled out after the dip and rolled it formed drips on the rim. Why fix the slurry instead of just rubbing this out? Keep reading. To fix this, I added water to decrease the specific gravity to 1.43. Then I added Epsom salts to induce thixotropy and gel it back to a creamy consistency. This time it went on evenly. Although the piece dries enough to handle in less than 30 seconds, it does take longer to dry completely because there is more water in the slurry. Adding CMC gum would also slow down drying, but it would be very tricky to get just the right amount (otherwise dripping could be worse than this). Consider a few of the advantages of thixotropic dipping glazes: They don't settle like a rock in the bucket, they don't go on too thick or in multiple thicknesses, they don't drip, and they don't dry too fast.

Can bone-dry ware be glazed too thickly?

Yes! When the specific gravity is 1.7.


This picture has its own page with more detail, click here to see it.

In testing to determine the best specific gravity (SG) for this Darvan-deflocculated glaze slurry (G2926B), I arrived at what I thought would be great: 1.7. For 2.5kg of glaze powder only 1100g (1100ml) of water is needed, half the normal amount. And the slurry flows well. There appears to be enough water to form a good bond with the body. But a one-second dip of a bone dry piece produces twice the desired thickness, it dries too slowly and it is running. So, what should the SG be? I'll keep increasing the water until I can induce some thixotropy to hold it in place (using Epsom Salts), and it goes on thinner in a quick dip. If thixotropy is difficult, I’ll add 1% bentonite to increase particle surface area. And, I'll document the results at each step for future reference (in my Insight-Live account). Of course, these are going to need help drying, either by preheating the ware or putting the pieces in a drier.

Specific gravities on three commercial glazes might surprise you


This picture has its own page with more detail, click here to see it.

The freshly opened transparent low-fire glaze on the left has a specific gravity of only 1.34 (a high water content compared to dipping glazes). Yet it is viscous and holds in place because they add a lot of gum. It needs three coats to go on thick enough and requires quite a bit of time to dry each one. Highly fritted transparent glazes need to be applied thin enough to be clear, thick enough to be glassy smooth but not too thick (to avoid clouding). Amaco likely targets the low specific gravity to enable good control of thickness. The center Potter's Choice glaze, is 1.52. And thus goes on nice and thick with each coat. That glaze likely contains lots of clay so little or no gelling agent (e.g. Veegum) is needed. The Celadon glaze on the right is in between, 1.46. Glaze manufacturers can produce at a broad range of specific gravities, they adapt the percentage of gum (e.g. Veegum and CMC gum) to impart the needed rheology and brushing characteristics.

Very low specific gravities on two commercial underglazes


Commercial underglazes with low specific gravities

This picture has its own page with more detail, click here to see it.

AMACO and Crysanthos. 1.26 (67.5% water) and 1.22 (68% water)! The former is well below their recommended specific gravity of 1.4 (it still paints well but needs more coats and more time to dry and apply them). The Crysanthos, although having a lower specific gravity is more viscous and goes on thicker (so it likely contains more gelling agent). When doing underglaze decorative brushwork it is important to get adequate thickness with each brush stroke, so a higher specific gravity is better. This may be reason enough to consider making your own (by adding stain powders to a base and using Veegum CER to gel the slurry, slow down its drying and harden it well at the dried state).

Inbound Photo Links


Terra cotta underglaze problem
This underglaze went on too thin: It’s specific gravity is too low

Links

Tests Rheology of a Ceramic Slurry
URLs http://en.wikipedia.org/wiki/Specific_gravity
Specific Gravity at Wikipedia
URLs https://www.smac.it/en/dettaglio.php?idprod=210
D-Glaze automatic glaze density controller
Maintains the glaze slurry density in existing glaze production lines.
Glossary Slip Casting
A method of forming ceramics. A deflocculated (low water content) slurry is poured into absorbent plaster molds. As it sits in the mold, usually 10+ minutes, a layer builds against the mold walls. When thick enough the mold is drained.
Glossary Viscosity
In ceramic slurries (especially casting slips, but also glazes) the degree of fluidity of the suspension is important to its performance.
Glossary Thixotropy
Thixotropy is a property of ceramic slurries of high water content. Thixotropic suspensions flow when moving but gel after sitting (for a few moments more depending on application). This phenomenon is helpful in getting even, drip-free glaze coverage.
Glossary Spray Glazing
In ceramic industry glazes are often sprayed, especially in sanitary ware. The technique is important.
Glossary Glaze Layering
In hobby ceramics and pottery it is common to layer glazes for visual effects. Using brush-on glazes it is easy. But how to do it with dipping glazes? Or apply brush-ons on to dipped base coats?
Glossary Deflocculation
Deflocculation is the magic behind the ceramic casting process, it enables slurries having impossibly low water contents and ware having amazingly low drying shrinkage
Glossary Rheology
In ceramics, this term refers to the flow and gel properties of a glaze or body suspension (made from water and mineral powders, with possible additives, deflocculants, modifiers).
Recipes G2926B - Cone 6 Whiteware/Porcelain transparent glaze
A base transparent glaze recipe created by Tony Hansen, it fires high gloss and ultra clear with low melt mobility.
Troubles Uneven Glaze Coverage
The secret to getting event glaze coverage lies in understanding how to make thixotropy, specific gravity and viscosity work for you
Troubles Powdering, Cracking and Settling Glazes
Powdering and dusting glazes are difficult and a dust hazard. Shrinking and cracking glazes fall off and crawl. The cause is the wrong amount or type of clay.
Media Thixotropy and How to Gel a Ceramic Glaze
I will show you why thixotropy is so important. Glazes that you have never been able to suspend or apply evenly will work beautifully.
Articles Understanding the Deflocculation Process in Slip Casting
Understanding the magic of deflocculation and how to measure specific gravity and viscosity, and how to interpret the results of these tests to adjust the slip, these are the key to controlling a casting process.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy