0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Rate | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Interaction | Oxide Molecular Formula | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Molecular Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Glaze Durability

Ceramic glazes vary widely in their resistance to wear and leaching by acids and bases. The principle factors that determine durability are the glaze chemistry and firing temperature.

Key phrases linking here: glaze durability, durability - Learn more

Details

Ceramic glazes vary widely in their resistance to wear (cutlery marking, scratching) and leaching by acids and bases. The principal factors that determine durability are the glaze chemistry and firing temperature. In the supply industry, technicians are accustomed to evaluating glazes by looking at their oxide chemistry and rationalizing the relationship between it and fired durability. Glazes having plenty of Al2O3 and SiO2, for example, are more durable (when they are melted properly). By contrast, potters tend to focus on the recipe. This is the reason that potters can be found using very non-functional glazes (often flux-saturated and therefore lacking in Al2O3 and SiO2) or firing them in a non-functional way (e.g. underfiring or overfiring).

Cutlery marking here is directly related to the chemistry of the glaze

Misconceptions are common. Many feel that just because a glaze looks melted, it is durable. Another common belief is that firing temperature is an indicator of durability; the higher it is fired, the more durable it will be. These beliefs, when coupled with the active traffic in glaze recipes online, greatly increase the chance that non-durable ware will be made. Sadly, a large proportion of online glazes are not durable and possibly not safe, even though they are published in fancy formats from apparently reputable sources. It is thus important to have a critical eye when looking at new recipes.

Another factor in why many people are using glazes of poor durability is the lack of appreciation of the basic science. The vast majority of glaze recipes available are for special-purpose colors and surfaces or are simply transparents with added colors and opacifiers. Quality transparent recipes, especially ones with documentation on how they were formulated and can be adjusted, are obviously less glamorous.

With some experience, it is possible to quickly judge durability issues when looking at a new glaze recipe. For example, at low temperatures (cone 06-04) boron is essential, so we expect to see a significant frit presence (or a natural boron source like Gerstley Borate), up to 80% is not uncommon. At high temperature, we expect to see no boron materials (feldspars, calcium carbonate, dolomite, wollastonite, and strontium carbonate are active melters there). At middle temperature, these do not melt well so they need help. That help is almost always boron, so you will see 10-40% frits or Gerstley Borate. Some middle temperature glazes use zinc and/or lithium in addition to or instead of boron (these are power melters). But it is important that melters not be in excess, as this will make the glaze leachable (since the SiO2 and Al2O3 percentages are pushed down).

At all temperatures, you should see clay in the recipe. 15-30% is typical (and needed for slurry suspension and dry hardness). At all temperatures, you should see silica, from 5-40%. If there is no clay or silica that is a red light if it is supposed to be a durable functional glaze.

It is possible to spot a leaching glaze just by looking at it

Testing durability is common sense. Expose it to an acid (e.g. the GLLE test) and to abrasion and scratching by hard materials.

Please see the Limit Formula and Recipe Logic glossary topics for more information on how to look at a formula and judge its balance.

There is a common misconception that the R2O:RO ratio in glazes is an indicator of their durability. However, as already noted, durability is much more about producing a well melted homogeneous glass (but not over-fluid) with minimal phase separation and surface crystallization, good body fit and absence of large amounts of easily dissolved colorants.

Related Information

Glossy blacks are best made adding a black stain to a quality base transparent


This picture has its own page with more detail, click here to see it.

The glaze on the left is called Tenmoku Cone 6 (a popular, and old, CM recipe). It is 20% calcium carbonate, 35% Custer feldspar, 15% OM4 Ball Clay and 30% silica, 10% iron oxide. If you have any experience with glaze you will note two things that a fishy here: There is no boron, lithia or zinc sourcing material. How can this melt enough at cone 6? It looks melted, but the ease of scratching it shows it is not. So, it appears that if we saturate an incompletely melted glaze with a lot of refractory brown colorant on a dark body the effect can be black. A better idea is the glaze on the right. We start with a stable, reliable base transparent, G2926B. Then we add 5% Mason 6666 black stain (stains are smelted at high temperatures, quenched and ground, they are inert and relatively safe). A bonus is we end up with a slurry that is not nearly as messy to use and does not turn into a bucket of jelly.

Can a cone 6 functional glaze having only whiting and feldspar melt enough?


This picture has its own page with more detail, click here to see it.

This flow test compares the base and base-plus-iron version of a popular CM recipe called "Tenmoku Cone 6" (20% whiting, 35% Custer feldspar, 15% Ball Clay and 30% silica, 10% iron oxide). Although iron is not a flux in oxidation, it appears to be doing exactly that here (that flow is just bubbling its way down the runway, the white one also fires to a glassy surface on ware). It looks melted in the tray on the right but notice how easily it is scratching on the tile (lower left). This demonstrates that looks can be deceiving. Cone 6 functional glazes always have some percentage of a power flux (like boron, lithia, zinc), otherwise they just do not melt into a hard glass. Maybe a glaze looks melted, but it has poor durability.

3% and 2% Zircopax added to G2926B cone 6 clear. Why?


This picture has its own page with more detail, click here to see it.

If you are interested in the most functional possible surface, consider a 2% zircon addition to your transparent glaze recipe (the outside glaze on these mugs is a copper blue, but that is not the one we are interested in). The clear glaze on the insides of these two identical cone 6 porcelain mugs has 3% and 2% zircon added. It is not being added to opacify, it is being added to toughen the surface and reduce the thermal expansion. The presence of the 2% zircon has not affected the gloss or transparency of the glaze on the right. However, the 3% on the left has opacified it just slightly and made the surface a little silky. So that is too much for this glaze (although it might be OK if the melt fluidity was higher).

Low fire glaze with the Al2O3 and SiO2 of a cone 6 glaze


This picture has its own page with more detail, click here to see it.

Look at how fluid G3879 is at cone 06 even though it has the Al2O3 and SiO2 of a cone 6 (or even cone 10 glaze)! It have found that glazes with lots of boron can tolerate amazingly high levels of Al2O3 and SiO2 and still melt very well. And they create many options to lower thermal expansion that would not otherwise be available. The G3806N recipe has the amazing ability to tolerate large additions of kaolin. Each addition sacrifices some melt fluidity but the glaze stays glossy and gets more durable (because of the increased Al2O3 and SiO2). And the thermal expansion drops even more. A highly melt fluid, super gloss with low thermal expansion is super difficult at cone 6, but here it is. The secret is high boron. From frits.

Links

Tests Glaze Leaching Test
Simple tests to evaluate the stability of a ceramic or pottery glaze against leaching metals in food or drink.
Glossary Cutlery Marking
Ceramic glazes that mark from cutlery are either not properly melted (lack flux), melted too much (lacking SiO2 and Al2O3), or have a micro-abrasive surface that abrades metal from cutlery.
Glossary Leaching
Ceramic glazes can leach heavy metals into food and drink. This subject is not complex, there are many things anyone can do to deal with this issue
Glossary Limit Formula
A way of establishing guideline for each oxide in the chemistry for different ceramic glaze types. Understanding the roles of each oxide and the limits of this approach are a key to effectively using these guidelines.
Glossary Transparent Glazes
Every glossy ceramic glaze is actually a base transparent with added opacifiers and colorants. So understand how to make a good transparent, then build other glazes on it.
Glossary Food Safe
Be skeptical of claims of food safety from potters who cannot explain or demonstrate why. Investigate the basis of manufacturer claims and labelling and the actual use to which their products are put.
Glossary Dishwasher Safe
Dishwasher safety is a concern in ceramic table ware, especially if the ware has been imported or made by a small company or potter.
URLs https://www.astm.org/d4236-94r21.html
ASTM D-4236 - Standard Practice for Labeling Art Materials for Chronic Health Hazards - It is not what you think!
ASTM D-4236 DOES NOT establish that a fired glaze is food-safe or resistant to leaching. It is a standard for evaluating and labelling chronic health hazards associated with using the art material itself. It "applies exclusively to art materials packaged in sizes intended for individual users of any age or those participating in a small group". It "concerns those chronic health hazards known to be associated with a product or product component(s) when it is present in a physical form, volume, or concentration that in the opinion of a toxicologist has the potential to produce a chronic adverse health effect". It also admits that "since knowledge about chronic health hazards is incomplete and warnings cannot cover all uses of any product, it is not possible for precautionary labelling to ensure completely safe use of an art product" (referring to safe use of the art product, not food safety of the fired pottery made from it). It is interesting that one manufacturer displays this warning on pages relating to dipping glazes and accessory products (which are used by manufacturers): "Safety Warning: Tableware producers must test all finished ware to establish dinnerware status, due to possible variations in firing temperature and contamination." That being said, some manufacturers do test glazes and underglazes for lead and cadmium release (e.g. using ASTM C927/C738 to meet FDA dinnerware guidelines). For them, ASTM D4236 is not the evidence presented for dinnerware-safety evidence; separate fired-glaze testing is. For example, one brushing glaze label specifically says its “Food Safe” designation comes from lead/cadmium-release testing under ASTM C738-94.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy