0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Rate | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition During Ceramic Firing | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | DTA Test | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | LAS Body | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | LOI-Adjust | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Interaction | Oxide Molecular Formula | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | TGA Test | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Molecular Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Fired Strength

Ceramics, by their brittle nature, have high compressive strength and unsurpassed surface hardness. Maximum fired strength can come at the expense of various working and fired properties, so testing is needed to reach a balance.

Key phrases linking here: fired strength - Learn more

Details

The fired strength of clays can be measured. The test is sometimes called M.O.R. or modulus of rupture, recognizing the fact that brittle ceramics fail suddenly (as opposed to others that fail after some plastic deformation). It is also known simply as tensile strength (because the point of failure is always where the sample is under the most tension). Ceramics perform much better under compressive strength testing than they do when stressed flexurally (compressive testing is more common in the structural ceramics industry).

Common sense suggests that the more vitrified a clay is, the stronger it will be. Likewise, we assume that higher temperatures produce stronger ware. However, the growth of mullite crystals in porcelain at high temperatures is the major reason for strength in vitrified bodies. However, other factors also contribute to fired strength (particle packing, vitrified vs. sintered, shape and surface properties, the presence of a glaze and its fit).

For glazeless vitrified ceramics, maturity is a key factor in achieving optimal fired strength. Testing is required since optimal strength may produce a body with more fired warping than desired. Strength may also drop off less than expected at lower levels of vitrification. Bodies that have been vitrified too much and have become glassy lose strength and become brittle. One reason is that over-maturity can detrimentally affect the development of mullite crystals (pyrophyllite is often added to porcelains to encourage better development of a mesh of long mullite crystals within the matrix). Lower temperature clay bodies can develop considerable strength at much higher porosities than you might expect. In fact, one of the strongest bodies we have ever tested was fired at cone 1 with around 3-4% porosity (more than 10,000 psi). However, in industry, good strength is achieved at much higher porosities than this, especially when body materials are very fine and the process densifies the matrix well. Wollastonite suppliers claim that additions of their material can greatly improve the fired strength of non-vitreous bodies. Thus, the optimal fired strength of a body is a product of a number of compromises involved with firing, forming, materials, glazing and the needed thermal expansion.

Ceramic is brittle, so any surface discontinuities (e.g. micro-tears made during forming from poor plasticity), cavities or pores (e.g. from material burned away during firing) or aggregate particles (coarse grog particles are often surrounded by micro-cracks as a product of drying and firing) provide places for cracks to propagate from. A body matrix can have coarser particles, but these must be complemented by a range of sizes that produce an overall matrix that has densified well during drying and firing.

When ceramics are glazed, a number of new factors must be considered. Glaze fit is very important. Crazing (thermal expansion too high) is a defect that produces micro-cracks that provide convenient sites for failure when stresses occur. Glazes under excessive compression (thermal expansion too low) shiver and can fail in a spectacular, and somewhat hazardous way. We have measured a 300% difference in fired strength between a poorly fitted glaze and a well-fitted one. A white stoneware, for example, measured about 2500 psi with a crazing glaze, while a well-fitted one measured 8000 psi. A simple way to test glaze fit is to age pieces for a few months and then break them. Ones with good fit, even if fired at low temperatures, will be much more difficult to break.

People accustomed to working only with vitrified bodies are often surprised at how strong sintered ones can be. Even though the latter lack the glass to cement particles together, when their particle size distributions are tuned to produce maximum density and surface contact their higher firing temperatures produce surprising strength. Low-fired ware can also be very strong if a low melting glass (like a frit) is incorporated into the recipe (e.g. Zero3 stoneware and porcelain).

Related Information

How much does clay shrink when bisque fired?


This picture has its own page with more detail, click here to see it.

Not much. These mugs were exactly the same height before a bisque firing to cone 06. The clay is a porcelain made from kaolin, feldspar and silica.

Which is stronger: Cone 10R mug or cone 03 mug?


This picture has its own page with more detail, click here to see it.

The mug on the left is high temperature Plainsman P700 (Grolleg porcelain). The other is Plainsman Zero3 fired at cone 03. Zero3 has a secret: Added frit which reduces the porosity of the terra cotta base (therefore increasing the density) dramatically. How? The frit melts easily at cone 03 and fills the interparticle space with glass, that glass bonds everything together securely as the piece cools. Although I do not have strength testing equipment right now, I would say that although the P700 mug likely has a harder surface, the Zero3 one is less brittle and more difficult to break.

Smash Pots to Make Better Ones!

Learn their dirty little secrets.


Breaking pottery to learn about its quality

This picture has its own page with more detail, click here to see it.

One dirty secret that a fracturing piece can tell you is: "I am weak, easily broken". I just filled two five-gallon pails and three boxes (I use a nylon hammer, and safety glasses, of course). Every type of clay and glaze I use. Every temperature. I started with a commercial Denby stoneware piece to get a feel for how quality ware should break. It becomes immediately evident which pieces are weak by the way they shatter (and how high a strength-bar commercial ware sets). Breaks with knife-like edges indicate strong body/glaze combos. Strong ware breaks into fewer pieces. Crazed ware is really weak. Ware with glaze compression (even if not shivering) explodes on impact. Low-fire ware can be very strong when glazes fit (and even better when it is fired to cone 03 or 02). High-fire ware can be surprisingly weak (if not vitreous or glaze fit is poor). This is an example where individual potters can take responsibility for ware quality and learn when to avoid DIFM thinking.

Vitrification can be obvious by simple visual inspection


This picture has its own page with more detail, click here to see it.

The unglazed surface of the left piece has a sheen; it is a product of glass development during firing to cone 6. That body is a 50:50 mix of a cone 8 stoneware and a low-fire earthenware red (a material that would normally be melted by this temperature). Together they produce this dense, almost zero-porosity (zero water absorption) ceramic. The unglazed surface on the right looks more like plaster, and it is absorbent, about 5% porosity. It is a mix of the same stoneware but with 50% ball clay. The refractory ball clay ensures that the stoneware, which was already inadequately vitreous, is even more so. As you can imagine, the left piece is far stronger.

To gauge strength: Break pieces often. Pay attention to what happens.


A broken slip cast cone 6 mug

This picture has its own page with more detail, click here to see it.

This is M340 casting, L3798H. The handle was just glued on with slip. I had questions about this new body. Are my glazes under compression? How well is the handle stuck on? Because I have broken so many pieces I know how their fracture pattern. It is a good sign when there are no fractures along the handle joins. And when the handle is the last to go. And when the item breaks into large pieces rather than shattering into small ones. Try doing this on some of your pieces and you might be surprised. Either by how strong they are. Or by how easily they break.

Low fire mug survives two-foot drop on to cement

In slow motion. This is Plainsman Snow clay, a super white burning dolomite body. Fired at cone 04. Although low-temperature ware is not as strong as stoneware it has more elasticity. Other than a tiny chip out of the base and handle, this mug still has the ring of strength. Where does this piece get all this strength? 1. It is glazed inside and out. 2. Glazes adhere well to this porous body, forming a deep interface. 3. The compression under which the glazes exist not only resists crazing but adds a lot of strength to the piece. Notice how it bounces onto the handle also!

Inbound Photo Links



Fired strength tester


The glaze broke the bottom off the pot!


The difference between vitrified and sintered


A vessel being forced apart by the pressure of a low expansion glaze inside

Links

Tests Fired Strength Round Bars
Materials Wollastonite
A source of CaO in glazes and a porcelain body material.
URLs http://en.m.wikipedia.org/wiki/Flexural_strength
Flexural Strength at Wikipedia
URLs https://www.eieinstruments.com/tiles_&_ceramics_testing_instruments/bending_strength_test/mor-testing-machine
MOR Testing Machine
Bending strength test. Compliance Standards: IS 13630 (Part - 6), ISO 10545 (Part-4)
URLs https://phys.org/news/2023-10-electron-rich-metals-ceramics-tough.html
Electron-rich metals can be added to ceramic to make it tough to crack
Glossary Sintering
A densification process occurring within a ceramic kiln. With increasing temperatures particles pack tighter and tighter together, bonding more and more into a stronger and stronger matrix.
Glossary Vitrification
A process that happens in a kiln, the heat and atmosphere mature and develop the clay body until it reaches a density sufficient to impart the level of strength and durability required for the intended purpose. Most often this state is reached near zero p
Glossary Restaurant Ware
If you are a potter and want to make restaurant ware, read this. Many of the things you already think you know will mislead you in this type of venture.
Minerals Mullite
Mullite (3Al₂O₃·2SiO₂) is a naturally occurring aluminum silicate crystalline mineral. It forms in h

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy