0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Rate | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition During Ceramic Firing | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | DTA Test | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | LAS Body | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | LOI-Adjust | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Interaction | Oxide Molecular Formula | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | TGA Test | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Molecular Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Porcelaineous Stoneware

In ceramics, porcelains lack plasticity and fire to high density with white, glassy surface. Stonewares are plastic and fire cream to brown and lower density, Porcelaineous stoneware are between these two.

Key phrases linking here: porcelaineous stoneware - Learn more

Details

Conceptually, a high temperature white porcelain could have recipe of 45:30:25 kaolin:feldspar:silica (typically high quality kaolin is employed and a bentonite addition is also needed to augment plasticity). It would fire dense, with zero porosity. If the kaolin is low in titanium and iron it could also be translucent. If the kaolin and feldspar and low in iron it could fire super white.

A stoneware could be something like 60:20:20 ball clay:feldspar:silica. There is more clay, and that clay is much more plastic than kaolin. There is less feldspar so it vitrifies less, perhaps having a porosity of 1-2%. It is thus less prone to warping in the kiln. And has zero fired translucency. There is less silica because the ball clay contains a percentage naturally. Often significant iron content in the ball clay can be tolerated, producing a body that fires tan or even brown. An important difference is that the stoneware has much less expensive materials. And it is much easier to form and dry. And easier to fit glazes to. It can fire anywhere from bone to brown, but for many types of ware that are completely glazed, the body color is not a big issue. Or, the iron in the body bleeds into the glaze providing an attractive aesthetic. Typically, the raw materials are industrially processed at 200 mesh particle size, however some producers can tolerate more coarsely ground clay. When this is the case, fired density and strength normally suffer somewhat.

Porcelaineous stoneware is somewhere between these two, I believe the term is best understood from the context of data, produced by experience in testing many types of bodies, measuring their physical properties and understanding these in terms of their recipes and firing circumstances. This perhaps a somewhat 'fuzzy' concept is betrayed by the variety of ways it can be spelled. But we can generalize that porcelaineous stoneware would typically always be using 200 mesh materials. "Porcelaineous" could mean that it needs to fire whiter. This could be accomplished by using lower iron ball clays (or by a mix of ball clay and kaolin). "Porcelaineous" could mean that it needs to be more vitreous than the stoneware, having a denser and more glassy surface or have more durability, hardness or strength. This could be accomplished by raising the feldspar to 25 or 30 (at the expense of the clay). "Porcelaineous" could also mean that a smoother plastic material is needed to create finer detail or produce a smoother fired surface. "Porcelaineous" could also mean that a producer can afford to spend some extra money on the body to achieve a combination of smoothness, whiter firing and better durability (at the cost of some workability).

All sorts of other materials are used in porcelains and stoneware, but this is a conceptual explanation of the differences. The whole topic is quite subjective. Many available clays are not really ball clays or kaolins, they are natural mixes of multiple clay minerals as well as feldspar and quartz. These are commonly employed in stonewares but much less likely to be used in porcelaineous stonewares (unless very finely ground). Fireclays are also often used in stonewares, but because they have coarser particle sizes, would not be employed in porcelaineous stonewares. Another factor to consider in terminology. People often refer to "vitreous stoneware", on doing that there may or may not be referring to porcelaineous stoneware (the term vitrification is not really a state but a process).

Related Information

A Super Plastic Stoneware Made With Two Materials

This mix showcases stoneware's advantages over porcelain


Feldspar/ball clay stoneware fits glazes, porcelain does not

This picture has its own page with more detail, click here to see it.

Left: 65% #6Tile kaolin and 35% nepheline syenite. Although it has great plasticity and fires white, it crazes the glaze and has 1% fired water absorption (using the SHAB test).
Right: 65% M23 Old Hickory ball clay (similar to OM#4) and 35% nepheline syenite (feldspar would also work). The glaze fits, the body fires very dense (zero porosity), and plasticity is fantastic!
The body on the left needs a 20% silica addition (to stop the crazing) and more nepheline (to reduce porosity to porcelain levels). The remaining 40% kaolin will not be nearly enough for a workable plasticity (so bentonite will be needed). The body on the right does not need fixing; it works as is. Many feel that stoneware body recipes must be built on a feldspar-containing base clay having pottery plasticity (adding ball clay, kaolin, feldspar and silica and ending up with needlessly complicated recipes). But ball clay is a base; all it needs is a non-plastic filler (to cut plasticity and therefore drying shrinkage) and a flux to vitrify it - feldspar or nepheline fills both roles.

Of course, this stoneware does not fire as white. But do you need white? Glazes will fire brightly colored on this surface. And cleaner ball clays are available in many areas (even ball clays intended for casting will be plastic enough). It is also worth considering the use of a white engobe.

OM4 Ball clay fired from cone 10R (top), 10 down to 4 (downward)


This picture has its own page with more detail, click here to see it.

Ball clays are normally refractory, none of these are vitrified to any extent. The cone 10R bar is yellow because it is stained by the soluble salts present in the material. These are very typical of what most ball clays look like.

Four North American ball clays fired at high temperature


This picture has its own page with more detail, click here to see it.

The top bars went to cone 10R, the others are cone 11 and 10 oxidation (downward from top). They are Gleason, Spinks Blend, OM#4 and NP Blend. It is amazing now similar different ball clays fire in the kiln. Clearly, soluble salts are an issue with all of them (the brownish scum). These bars are much cleaner on the backsides (since the solubles were left on the surface on the fronts during drying). The drying shrinkages, plasticities and fired maturities are also all remarkably similar.

Links

Glossary Vitreous
The fired state of a ceramic when sufficient heat in the kiln has produced the density and strength common, and expected, in stonewares and porcelains.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved