0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Rate | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition During Ceramic Firing | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | DTA Test | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | LAS Body | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | LOI-Adjust | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Interaction | Oxide Molecular Formula | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | TGA Test | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Molecular Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Oxide Interaction

In ceramic glazes each oxide generally makes a specific contributions to the melting and freezing behavior of the glaze. However interactions are also important.

Key phrases linking here: oxide interaction - Learn more

Details

In a glaze melt, oxides do not act alone, they interact. For example, while one material might not melt well by itself, when combined with others the mix as a whole can melt at a significantly lower temperature than any of the ingredients in the mix. Cornwall stone is an example, by itself it does not melt enough to even be a glaze at cone 10, but a glaze can be made using this material in combination with kaolins, silica, etc. Oxides that are even refractory by themselves can be powerful fluxes in combination with silica and alumina, a good example is the material calcium carbonate. By itself it is completely refractory and yet at cone 8-10 it is the principal flux in stoneware glazes. Thus, due to interaction, the function of the oxide is changed completely.

Related Information

Two Cornwall Stone shipments compared to two substitutes


This picture has its own page with more detail, click here to see it.

This is a cone 11 oxidation melt flow test. Shown (left to right):
-A new shipment of Cornwall Stone 2011
-L3617 Digitalfire calculated substitute recipe
-An older Cornwall shipment
-The H&G substitute 2011 (far right, mislabelled on the picture).
These do not flow well here, a small frit addition was later employed to better compare them. However they have melted enough to see some differences in whiteness and degree of melt. Notice the L3617 is more like the old Cornwall Stone than the new Cornwall is.

Calcium carbonate and dolomite test bars:

These demonstrate how refractory these materials are


This picture has its own page with more detail, click here to see it.

Examples of calcium carbonate (top) and dolomite (bottom). Both are mixed with 25% bentonite to make them plastic enough to form test bars. They are fired to cone 9. In spite of the significant bentonite present, which melts at this temperature, both of these bars are very porous and refractory, even powdery. However, put either of these in a glaze batch with other ceramic minerals, and they interact strongly to become fluxes!

Frits melt so much better than raw materials


Frits, talc, feldspar melting

This picture has its own page with more detail, click here to see it.

Feldspar and talc are both flux sources (glaze melters), they are common in all types of stoneware glazes. But their fluxing oxides, Na2O and MgO, are locked in crystal structures that neither melt early or supply other oxides with which they like to interact. The pure feldspar is only beginning to soften at cone 6. Yet the soda frit is already very active at cone 06! As high as cone 6, talc (the best source of MgO) shows no signs of melting activity at all. But a high-MgO frit is melting beautifully at cone 06! The frits progressively soften, starting from low temperatures, both because they have been premelted and have significant boron content. In both, the Na2O and MgO are free to impose themselves as fluxes, actively participating in the softening process.

Ionic Forces Chart


This picture has its own page with more detail, click here to see it.

Cations having high charges and small radiuses (and thus high field forces like boron and silicon), are network formers. Network modifiers have small charges, large radiuses and a big coordination number for oxygen ions. While considering ions as rigid spheres is an over-simplified way to describe reality, it has still proven useful to describe characteristics of each. For instance lithium has a ionic radius smaller than sodium and so it can locate into smaller cavities. The ionic field force of lithium is also stronger than sodium and it is essentially non-directional, thus it more easily produces crystals of a separate phase. Alkaline earth elements locate into cavities of the network as well, but they have double charges and thus act like a bridges between two oxygen ions (preventing the three-dimensional network from being fully destroyed). Moreover bonds between alkaline earth ions and oxygen are stronger than alkaline so we observe neither a rapid decrease in viscosity or a significant increase of the thermal expansion coefficient. It is notable that for similar molar percentages, frits containing magnesium crystallize more easily than frits containing calcium.

Aluminum, titanium and zirconium are classified as intermediate glass formers because they have a strong four-way coordination for oxygen ions, like silicon. Thus, for these oxides, we do not observe any interruption of the three-dimensional silicate-based network. For a better understanding consider more details about aluminum, boron, zirconium and titanium.

Aluminum: Usually aluminum shows a four-way coordination when it acts as a glass former, tetrahedrons are linked to four oxygen atoms while the local excess of negative charge is counterbalanced by an alkaline cation placed close to the aluminum ion. Thus additions of aluminum to a glass help to stop alkaline ions from breaking the three dimensional network of the glass. This produces the characteristic lower melt fluidity and tendency to crystallize and also reduces the thermal expansion and thermal stability. One downside to alumina is that it contributes to a higher viscosity of frit batches during melting (in the furnace tank) making homogenization more difficult. Usually the percentage of aluminum oxide is in the range 4 – 12%.

Boron: Boron is a basic component of frits yet its characteristics are so peculiar that it cannot easilly be compared to other elements. Boron, like aluminum, exhibits a four-way coordination when forming a glass network (being in the center of a tetrahedron of oxygen ions). This is possible only when the molar alkaline percentage is less than 30-40% because above this limit boron has three-way coordination, forming triangles.

Another peculiar characteristic is that boron is not just dispersed as tetrahedrons or triangles in the network of silica tetrahedrons. Rather it forms boric groups, containing from 3 to 5 boron atoms and the groups are randomly dispersed in the glassy matrix. However single BO3 triangles and BO4 tetrahedrons are always present. For quenched frits the presence of these groups is likely minimal but we can presume they form again when glazes containing the frit are fired (there are experimental evidences demonstrating this).

Boron oxide is an important component of low melting frits because it increases fusibility without a proportional increase in thermal expansion. Moreover boron oxide and sodium borate, due to their low melting point, are useful during smelting of frits because they form a glassy matrix early and act as catalysts in the melting and dissolving of other materials.

Zirconium - Titanium: Their influence on surrounding oxygen ions is very strong and scarcely directional so their solubility in frits is poor. Their solubility in glass and actions as glass formers are proportional to temperature. In quenched frits they remain in the dissolved in the glassy matrix but when we fire them again (within a glaze), these oxides easily precipitate crystal compounds.

Links

Oxides CaO - Calcium Oxide, Calcia
Materials Cornwall Stone

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy