0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Rate | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition During Ceramic Firing | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | DTA Test | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | LAS Body | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | LOI-Adjust | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Interaction | Oxide Molecular Formula | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | TGA Test | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Molecular Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Phase Separation

Phase separation in glaze melts creates microscopic discontinuities that affect transparency, color variegation, matte surfaces, and reactive glaze effects.

Key phrases linking here: phase separations, phase separation, phase changes - Learn more

Details

Phase separation occurs when a molten glaze does not remain a single chemically uniform liquid but separates at the microscopic scale into two or more glassy phases of slightly different composition. During cooling, these phases may form droplets, interconnected networks, or domains dispersed within one another. Although the glaze appears solid after firing, the final glass may contain countless microscopic discontinuities created during the melt or cooling process.

These discontinuities arise because certain oxide combinations are only partly compatible in a silicate melt. Instead of remaining fully dissolved in one homogeneous glass, portions of the melt separate into regions richer in particular oxides. This often develops late in firing or during cooling, when melt mobility decreases and local chemistry differences become more significant. In some cases, incomplete dissolution of batch materials or delayed interaction between decomposing particles can encourage the process.

Colorants and opacifying oxides may preferentially concentrate in one phase rather than another. As a result, phase separation can produce variegation, clouding, soft mottling, or subtle color shifts because different phases may have different refractive indices, viscosities, and capacities to host coloring ions.

Phase separation is often undesirable in glazes intended to be crystal clear. The internal interfaces between phases scatter light, reducing transparency and producing milkiness or haze even when no crystals are present. This is one reason some high-boron transparent glazes appear slightly cloudy despite being fully melted.

In industrial glassmaking, phase separation is carefully controlled because it affects optical clarity and durability. Increased alumina often helps stabilize the glass network and suppress separation, although excessive alumina can also promote devitrification if cooling conditions allow crystal growth. Sodium can improve melt homogeneity by increasing fluxing action, but excessive Na₂O also raises thermal expansion and may create fit problems in ceramic glazes.

In ceramics, however, phase separation is not always undesirable. Many so-called reactive glazes depend on controlled microscopic heterogeneity to develop visual depth and complexity. Sanitary ware glazes, such as those used on sinks and toilets, are formulated to remain highly homogeneous, producing smooth, durable, fully transparent glass with minimal internal discontinuity.

Some matte glazes are partly influenced by phase separation. In dolomite mattes, for example, MgO encourages limited immiscibility in the melt and can also promote crystal development during cooling. The matte effect usually results from both microscopic phase separation and fine crystal precipitation rather than phase separation alone.

Titanium and rutile additions strongly encourage discontinuity because they reduce glass uniformity and often stimulate crystal nucleation. In fluid iron-bearing glazes, rutile can intensify local segregation of iron and titanium, contributing to streaking effects such as blue rivulets suspended in amber glass. In these cases, the visual effect often involves both phase separation and selective crystallization acting together.

Related Information

Phase separation close-up

The power of modern phone cameras


This picture has its own page with more detail, click here to see it.

This reduction stoneware glaze is producing white streaks on some pieces (left center). The body is a coarse iron stoneware. A magnification is needed to better explain this.

It is 2025, many smartphones now have dedicated macro lenses and can be held as close as a 1 centimeter. They automatically sense placement and switch to using the macro lens. Of course, the phone must be held rock steady and good lighting is essential. If you are a doubter of what they can produce, look at the two magnifications on the right. On the top one, the white streak is clearly visible, floating in a sea of phase-separated glass patterned by earlier-escaping bubbles. The extreme magnification on the bottom right appears to implicate tiny crystals growing in an area where late bubbles have escaped, changing the pattern of phase separation. This doesn’t yet explain the cause, but it is valuable information courtesy of a macro lens.

A glaze whose visual effect is partly a product of phase separation


This picture has its own page with more detail, click here to see it.

Example of a rutile-iron stained glaze. Rather than crystallizing to form the visual effect, the rutile is forming a phase separation that produces the streaking blue in the amber background glass.

Variegation and phase separation with about 5% rutile


This picture has its own page with more detail, click here to see it.

The glaze is a dolomite matte. G2571A, fired to cone 10R. High-fire reduction is among the best processes to exploit the variegating magic of rutile.

Micrograph of phase separation in a glaze


This picture has its own page with more detail, click here to see it.

Two glazes of the same chemistry:

But supplied by different sets of materials


This picture has its own page with more detail, click here to see it.

These two specimens are the same terracotta clay fired at cone 03 in the same kiln. The glaze on the left combines 30% frit with five other materials. The one on the right mixes 90% frit with one other material (kaolin). Ulexite is the main source of boron in #1, it decomposes during firing, expelling 30% of its weight as gases, mostly CO2, forming micro-bubbles. Each of the six materials in that recipe has its own melting characteristics; their interaction creates a non-homogeneous glass containing phase separations (discontinuities) that affect the fired surface. In the fritted glaze, by contrast, all the particles soften and melt in unison and produce no gas. Notice that it has also interacted with the body, fluxing and darkening it (thus forming a better interface). And it has passed (and healed) more of the bubbles from the body.

Links

Glossary Crystalline glazes
A type of ceramic glaze made by potters. Giant multicolored crystals are grown on a super gloss low alumina high zinc glaze by controlling multiple holds and soaks during cooling in the kiln.
Glossary Matte Glaze
Random material mixes that melt well overwhelmingly want to be glossy, creating a matte glaze that is also functional is not an easy task.
Glossary Reactive Glazes
In ceramics, reactive glazes have variegated surfaces that are a product of more melt fluidity and the presence of opacifiers, crystallizers and phase changers.
Glossary Magnesia Matte
Magnesia matte ceramic glazes are “microstructure mattes” while calcia mattes are “crystal mattes”. They have a micro-wrinkle surface that forms from a high viscosity melt and microscopic phase separation, both of which prevent levelling on freezi
Glossary Melting Temperature
The melting temperature of ceramic glazes is a product of many complex factors. The manner of melting can be a slow softening or a sudden liquifying.
Glossary Rutile Blue Glazes
A type of ceramic glaze in which the surface variegates and crystallizes on cooling in the presence of titanium and iron (usually sourced by rutile)
Recipes G2571A - Cone 10 Silky Dolomite Matte glaze
A cone 10R dolomite matte having a pleasant silky surface, it does not cutlery mark, stain or craze on common bodies
Properties Glaze Variegation
Articles High Gloss Glazes
A transcript of a presentation at the 3rd Whitewares conference at Alfred University in the spring of 2000 by Richard Eppler.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy