0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Substitution | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Formula | Oxide Interaction | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silica:Alumina Ratio | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Dinnerware Safe

In pottery, the terms dinnerware safe and food safe, are not the same. Perhaps the best way to understand the former is to consider what the opposite might be.

Key phrases linking here: dinnerware safe - Learn more

Details

Dinnerware safety of glazes means something different in industry than it does in pottery or hobby ceramics. For the former, it is about conservative formulations that work well in high-production machinery and kilns, that produce glassy smooth and easy-to-clean surfaces. It is about commercial testing labs with well-defined procedures to flag leaching, crazing, pitting, staining, etc. In pottery, suppliers use the term more loosely. No potters attach "Dinnerware Safe" stickers to their ware.

Dinnerware safe is not the same as the official term Foodsafe: The latter is regulated by the FDA and regulates the release of lead or cadmium from glazes. The regulation does not require that glazes be lead or cadmium-free, just that they do not leach them. In pottery, we tend to think of food safety as, at a minimum, not containing lead. But we do use stains containing all sorts of heavy metals. And the commercial glazes we buy are full of them.

While there is no industry standard or official symbol that signifies the dinnerware safety of a bottle of commercial glaze sold at ceramic suppliers, some manufacturers have designed their own symbol and labelling. On their websites they explain what these mean. Typically, the term refers to chemical durability and freedom from surface micro-textures that could trap bacteria or make it difficult to clean. The term is sufficiently clear and companies test it with enough confidence that they even promise to back any customer that is targeted by litigation. That being said, it is difficult to imagine that they could indemnify users given all the ways their products can be misused and all the issues surrounding their interactions when layered.

These commercial glazes don't leach on their own, but when layered like this pronounced leaching, the white, has occurred with lemon juice overnight

So this all means that it is up to you, the potter, to test your ware. The term "dinnerware safe" embodies the ability of a glaze to withstand exposure to acidic and base liquids is a basic expectation (often referred to as surface durability). Coffee, acidic fruits and coke can degrade surfaces - we can be sure glaze manufacturers test for these exact liquids. That means you can do it also (e.g. the GLLE test).

Added reason for doing your own testing comes with the realization that the "Non-Toxic" seal on jars of glaze, which refers to ASTM D-4236, does not likely mean what you think.

The term Dinnerware Safe can also be understood by considering its opposite. For example, to make a glaze that leaches heavy metal one would use a high percentage (e.g. 20%+) of heavy metal oxide (or even stain), make it highly melt fluid (having inadequate SiO2 glass former and Al2O3 stabilizer) and cool it slowly in the firing to crystallize out the metals in concentration. Further destabilization could be accomplished by layering all manner of different products, especially ones containing copper, to produce interactions.

Potters who make their own glazes are the ones who can speak with greatest assurance about their ware. Glazes that do not contain any potentially toxic ingredients are no danger, even if they leach (from a liability standpoint). This is because potters know the recipes of the glazes they mix. As noted above, practical testing for leaching is easy to do. And testing for crazing and surface textures that resist cleaning is equally easy.

Related Information

Feeling good about the glazes we use on functional surfaces


Val's Turpquoise glaze chemistry

This picture has its own page with more detail, click here to see it.

The chemistry of the popular cone 6 Val's Turquoise glaze surprised a customer recently (when she was comparing the Gerstley Borate and Gillespie Borate versions). Here is what she said initially about using this on food surfaces:

"I’ve noticed the alumina is below the suggested limits. I have read that too low alumina can cause a glaze to be more prone to leaching, especially with the addition of copper carb. I’ve soaked samples in vinegar and lemon juice. I’ve also run pieces through the dishwasher several times with no visible changes."

Her concerns about this chemistry anomaly are valid. This glaze has no clay, that is very strange, clay sources vital Al2O3 that imparts durability. The little Al2O3 there is being sourced by lots of feldspar, that is a red light for crazing when little MgO is present (from talc or dolomite). Of course, even if this glaze does leach, the copper is not going to hurt anyone. However, if another heavy metal pigment were added the Cu could destabilize it enough to make toxicity a concern.

Her final comment was this: "I never want a customer coming back to me with a faulty pot. I just want to do everything within my power to make the best ware that I can - which includes a durable, reliable and functional glaze."

Links

URLs https://www.astm.org/d4236-94r21.html
ASTM D-4236 - Standard Practice for Labeling Art Materials for Chronic Health Hazards - It is not what you think!
ASTM D-4236 DOES NOT establish that a fired glaze is food-safe or resistant to leaching. It is a standard for evaluating and labelling chronic health hazards associated with using the art material itself. It "applies exclusively to art materials packaged in sizes intended for individual users of any age or those participating in a small group". It "concerns those chronic health hazards known to be associated with a product or product component(s) when it is present in a physical form, volume, or concentration that in the opinion of a toxicologist has the potential to produce a chronic adverse health effect". It also admits that "since knowledge about chronic health hazards is incomplete and warnings cannot cover all uses of any product, it is not possible for precautionary labelling to ensure completely safe use of an art product" (referring to safe use of the art product, not food safety of the fired pottery made from it). It is interesting that one manufacturer displays this warning on pages relating to dipping glazes and accessory products (which are used by manufacturers): "Safety Warning: Tableware producers must test all finished ware to establish dinnerware status, due to possible variations in firing temperature and contamination." That being said, some manufacturers do test glazes and underglazes for lead and cadmium release (e.g. using ASTM C927/C738 to meet FDA dinnerware guidelines). For them, ASTM D4236 is not the evidence presented for dinnerware-safety evidence; separate fired-glaze testing is. For example, one brushing glaze label specifically says its “Food Safe” designation comes from lead/cadmium-release testing under ASTM C738-94.
Glossary Food Safe
Be skeptical of claims of food safety from potters who cannot explain or demonstrate why. Investigate the basis of manufacturer claims and labelling and the actual use to which their products are put.
Tests Glaze Leaching Test
Simple tests to evaluate the stability of a ceramic or pottery glaze against leaching metals in food or drink.
Tests 300F:Ice Water Crazing Test
Ceramic glazes that do not fit the body often do not craze until later. This progressively stresses the fit until failure point, thus giving it a score

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy