0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Rate | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition During Ceramic Firing | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | DTA Test | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | LAS Body | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | LOI-Adjust | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Interaction | Oxide Molecular Formula | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | TGA Test | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Molecular Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Residual Quartz

Residual quartz is the crystalline quartz that remains undissolved in a fired ceramic body. It is not the same thing as the total SiO2 reported in a body chemistry. Much of that SiO2 may be chemically combined in clay minerals, feldspars and other silicates, and some quartz added to the recipe may dissolve into the developing glass phase during firing. Residual quartz refers specifically to the quartz crystals that survive the firing.

This distinction is extremely important in porcelain and stoneware because residual quartz can have a major influence on the thermal expansion of the fired body. Quartz has a relatively high thermal expansion, and it also undergoes the well-known alpha-beta quartz inversion at about 573°C. Thus, a body containing appreciable residual quartz normally has a higher overall thermal expansion than the same body after more of that quartz has dissolved into the glassy phase.

This is one reason silica is deliberately added to many porcelain recipes. A typical porcelain might contain 20–30% added silica, much of it as quartz. Although some goes into solution during firing, enough normally remains to act as a relatively refractory aggregate within the fired matrix. That residual quartz helps establish the thermal expansion of the body and can therefore be important to glaze fit. Removing the silica from a porcelain recipe does not simply remove an inert filler; it can dramatically lower body expansion and make a previously fitting glaze craze.

The amount of residual quartz is not determined by the recipe alone. It depends on particle size, firing temperature, firing time, the amount and chemistry of the liquid phase and the degree of vitrification. Fine quartz dissolves more readily than coarse quartz. Higher temperatures and longer firing generally permit more quartz to enter the melt. A body that is fired repeatedly can therefore continue to lose residual quartz as additional silica dissolves into the glass phase.

This helps explain why refiring can change glaze fit. If a porcelain or vitreous stoneware is already highly fired, another firing may dissolve additional quartz without producing an obvious change in appearance or porosity. Yet the fired body's thermal expansion can decrease. A glaze that was adequately compressed after the first firing could thus move closer to crazing after subsequent firings. Highly vitreous bodies, including sanitaryware and porcelains subjected to repair firing, deserve particular attention in this respect.

Residual quartz also presents a mechanical complication. Individual quartz grains change dimensions abruptly as they pass through the quartz inversion. If grains are large, the surrounding glassy matrix must accommodate that movement, creating localized stresses and potentially microcracking. This is why coarse silica particles can contribute to dunting and why quartz particle size matters, not just the percentage in the recipe. Nevertheless, ceramic bodies can contain substantial quartz without simply cracking apart around every particle: particle size, distribution, matrix elasticity, porosity and the compressive stresses that develop during cooling all influence whether those stresses become destructive.

Stonewares commonly contain residual quartz even when no silica has been intentionally added. Natural clays often contain quartz as an accessory mineral, sometimes in significant amounts. Thus two stoneware bodies having similar porosity and similar calculated chemistry can have quite different thermal expansions because their mineralogy and residual quartz contents differ.

For this reason, calculated oxide chemistry alone cannot reliably predict the thermal expansion of a fired clay body. Glaze expansion calculations are useful because glazes are largely glassy. Fired bodies are multiphase materials containing glass, mullite and other crystals, residual quartz and sometimes cristobalite. Their thermal expansion is therefore a product of the proportions, particle sizes and thermal behavior of all of these phases.

A useful way to think about residual quartz is this: silica in the recipe is a starting quantity; residual quartz is what survives the firing. It is the latter that matters most when considering quartz inversion, body thermal expansion and its contribution to glaze fit.


PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy