0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Rate | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition During Ceramic Firing | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | DTA Test | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | LAS Body | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | LOI-Adjust | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Interaction | Oxide Molecular Formula | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | TGA Test | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Molecular Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Surface Tension

In ceramics, surface tension is discussed in two contexts: The glaze melt and the glaze suspension. In both, the quality of the glaze surface is impacted.

Key phrases linking here: surface tension - Learn more

Details

In ceramics, the issue of surface tension is most evident in two areas: The glaze melt and slurry rheology.

Surface Tension in Glaze Melts

When a glaze is fired, it melts to form a molten silicate glass. This melt exhibits surface tension, a thermodynamic property that reflects the tendency of the liquid to minimize its surface area. In ceramic glazes, surface tension plays a key role in how the melt wets the clay body, releases gases, and levels during firing and cooling.

Wetting and Spreading: Low surface tension promotes wetting of the clay body and allows the glaze to spread more readily across the surface. High surface tension resists wetting and encourages the melt to contract into thicker regions, contributing to edge pull-back, beading, crawling, and poor coverage.

Bubble Release: Assuming sufficient melt viscosity, surface tension governs how easily gas bubbles rupture at the melt surface. Low surface tension enhances merging and makes bubble films easier to break. High surface tension strengthens the bubble skin, allowing bubbles to persist, reseal, or remain trapped.

Levelling and Surface Smoothness: Surface tension provides the driving force for surface smoothing. However, the extent and rate of levelling are controlled primarily by viscosity (melt mobility). A glaze with high surface tension but low viscosity can still level well, while a glaze with low surface tension but high viscosity may freeze before smoothing is complete. Surface tension helps explain why some glazes pull away from sharp edges while pooling in recesses.

Surface tension in silicate melts is strongly influenced by oxide chemistry, as different oxides alter the structure and ionic bonding of the glass network. A critical caution: many oxides affect surface tension indirectly by changing viscosity and melt structure at the same time, so practical glaze behavior cannot be predicted from surface tension alone.

Oxides commonly associated with higher surface tension (assuming similar melt viscosity, approximate, system- and concentration-dependent). Rightward have higher surface tension and are thus associated with increased melt stiffness, reduced wetting and bubble mobility:
MgO, Al2O3, ZrO2, ZnO, CaO, SnO2, BaO, SrO

Oxides commonly associated with lower surface tension (lowest surface tension rightward; these generally promote wetting, improve levelling, enhance bubble merging and rupture, more gloss):
PbO, B2O3, K2O, Na2O, Li2O

SiO2 forms the glass network and usually raises viscosity strongly, but its effect on surface tension is moderate rather than extreme.

Fe2O3 effects vary strongly with oxidation state, concentration and firing atmosphere.

ZnO is chemically distinctive in that it can function as a strong flux while also increasing melt viscosity, modifying surface behavior and contributing to matte or semi-matte effects in some systems.

ZnO is unusual because it often acts as a flux while simultaneously stiffening melt behavior in certain systems. It can increase crystallization tendency, promote matte surfaces and alter bubble persistence. Its effect is highly composition-dependent.

Practical Implications:

High surface tension + high viscosity: Beading, crawling, poor bubble escape, pinholing, incomplete healing, matte or uneven surfaces.
Low surface tension + low viscosity: Good wetting, smooth levelling, glossy surfaces, good defect healing, possible running.
High surface tension + low viscosity: Can still level well, but may show edge pullback, thick/thin variation, and bubble persistence.
Low surface tension + high viscosity: Implies good coverage, satin surfaces, incomplete levelling if cooling is rapid.

Surface tension is strongly implicated in glaze blistering. Blisters happen where the molten glaze resists bubble rupture at the surface. These or their unhealed remnants often survive to the fired piece when gas pressure inflates the bubble, surface tension maintains the film and viscosity prevents rapid healing after rupture. Strangely, glazes of a more fluid melt can exhibit this problem more, the melt is mobile enough for bubbles to expand, but the surface remains strong enough to hold them. The solution can be a slower cooling through the range at which increasing temperature-induced viscosity has the power to rupture the film. Replacing some higher-surface-tension oxides with lower-surface-tension fluxes often improves blister resistance more effectively than simply increasing melt fluidity.

Surface Tension of Glaze Slurries

On flat surfaces, glaze laydown is not normally an issue, but slurries are suspensions and can resist adhesion and give poor coverage on irregular surfaces (e.g. acute angles, incised or stamped decoration or labelling). Surfactants are available to reduce the surface tension of aqueous glaze systems, they deagglomerate particles and help their homogeneous dispersion over the surface. Polyethylene glycol and Glycerin are considered wetting agents also.

Related Information

These two transparent glazes are opposites:

In melt fluidity and surface tension


Melt flow test demonstrates surface tension

This picture has its own page with more detail, click here to see it.

This cone 04 flow tester compares two commercial low-fire transparent glazes. Their different chemistry strategies are revealed by the shape of these melt flows. While 3825B appears to have the higher melt fluidity, it also has much higher melt surface tension. This is evident in the narrow, rope-like stream and the way the flow meets the runway at a high angle before pulling into a rounded bead. A, by contrast, spreads and wets the runway, meandering downward in a broad, flat and relatively bubble-free river.

This difference is important in low-fire ware because these glazes must pass far more gases and bubbles than high-temperature glazes. The lower surface tension of A aids bubble release and healing after bubbles break. A is Amaco LG-10. B is Crysanthos SG213 (Spectrum 700 behaves similarly, although flowing less). Both approaches have advantages and disadvantages and are worth testing in your application.

Surface tension differences between two glazes:

This simple test shows them best


This picture has its own page with more detail, click here to see it.

Both are low-fire transparents. In a melt fluidity (GBMF test) they flow similarly. But here, where the 10 gram ball of the dry glaze is simply melted down onto a square tile (a GBMF test), differences in surface tension are more clearly evident by the angle at which the edge of the glaze meets the tile.

The perfect storm of high surface tension and high LOI: Blisters.


This picture has its own page with more detail, click here to see it.

An example of how calcium carbonate can cause blistering as it decomposes during a fast firing in our electric kiln. This is a cone 6 borosilicate glaze with 15% calcium carbonate added (there is no blistering without it). Calcium carbonate has a very high loss on ignition (LOI), and for this early-melting glaze, the gases of its decomposition are still escaping after melting begins. Another factor is also involved: Although the glaze has good melt fluidity, bubbles survived till near the end of the firing, resisting rupture (likely because of the high surface tension of the melt). When the bubbles finally did burst, there was inadequate time for healing to occur.

The difference that caused blistering: Firing schedule!


This picture has its own page with more detail, click here to see it.

These are the same glaze, same thickness, Ulexite-based G2931B glaze, fired to cone 03 on a terra cotta body. The one on the right was fired from 1850F to 1950F at 100F/hr, then soaked 15 minutes and shut off. The problem is surface tension. Like soapy water, when this glaze reaches cone 03 the melt is quite fluid. Since there is decomposition happening within the body, gases being generated vent out through surface pores and blow bubbles. I could soak at cone 03 as long as I wanted and the bubbles would just sit there. The one on the left was fired to 100F below cone 03, soaked half an hour (to clear micro-bubble clouds), then at 108F/hr to cone 03 and soaked 30 minutes, then control-cooled at 108F/hr to 1500F. During this cool, at some point well below cone 03, the increasing viscosity of the melt becomes sufficient to overcome the surface tension and break the bubbles. If that point is not traversed too quickly, the glaze has a chance to smooth out (using whatever remaining fluidity the melt has). Ideally I should identify exactly where that is and soak there for a while.

Carbonate gassing can cause glaze blisters


This picture has its own page with more detail, click here to see it.

An example of how a carbonate can cause blistering. Carbonates produce gases during decomposition. This glaze (G2415B) contains 10% lithium carbonate, which likely pushes the initial melting temperature down toward the most active decomposition temperatures.

Blistering in a cone 6 white variegated glaze. Why?


This picture has its own page with more detail, click here to see it.

This glaze creates the opaque-with-clear effect shown (at cone 7R) because it has a highly fluid melt that thins it on contours. It is over fired. On purpose. That comes with consequences. Look at the recipe, it has no clay at all! Clay supplies Al2O3 to glaze melts, it stabilizes it against running off the ware (this glaze is sourcing some Al2O3 from the feldspar, but not enough). That is why 99% of studio glazes contain clay (both to suspend the slurry and stabilize the melt). Clay could likely be added to this to increase the Al2O3 enough so the blisters would be less likely (it would be at the cost of some aesthetics, but likely a compromise is possible). There is another solution: A drop-and-soak firing. See the link below to learn more. One more observation: Look how high the LOI is. Couple that with the high boron, which melts it early, and you have a fluid glaze melt resembling an Aero chocolate bar!

Inbound Photo Links



High and low melt surface tension: As demonstrated by two pure frits

Glaze dried with pinholes
Gummed dipping glazes can dry like this: How to fix it.

Links

Troubles Crawling
Crawling glazes pull into islands, leaving bare spots on the body. Asking yourself the right questions will surface the real cause and help you deal with the problem, not the symptoms.
Troubles Glaze Blisters
Questions and suggestions to help you reason out the real cause of ceramic glaze blistering and bubbling problems and work out a solution
Glossary Glaze Crawling
A ceramic glaze fault that occurs during firing of the ware, the molten glaze pulls itself into islands leaving bare patches of body between.
Glossary Glaze Blisters
Blistering is a common surface defect that occurs with ceramic glazes. The problem emerges from the kiln and can occur erratically in production. And be difficult to solve.
Glossary Glaze Bubbles
Suspended micro-bubbles in ceramic glazes affect their transparency and depth. Sometimes they add to to aesthetics. Often not. What causes them and what to do to remove them.
Glossary Melt Fluidity
Ceramic glazes melt and flow according to their chemistry, particle size and mineralogy. Observing and measuring the nature and amount of flow is important in understanding them.
Glossary Rutile Blue Glazes
A type of ceramic glaze in which the surface variegates and crystallizes on cooling in the presence of titanium and iron (usually sourced by rutile)
Glossary Fluid Melt Glazes
Fluid melt glazes and over-melting, over fired, to the point that they run down off ware. This feature enables the development of super-floss and cyrstallization.
Glossary Ceramic Glaze Defects
Ceramic glaze defects include things like pinholes, blisters, crazing, shivering, leaching, crawling, cutlery marking, clouding and color problems.
Articles A Low Cost Tester of Glaze Melt Fluidity
Use this novel device to compare the melt fluidity of glazes and materials. Simple physical observations of the results provide a better understanding of the fired properties of your glaze (and problems you did not see before).
Recipes G3806C - Cone 6 Clear Fluid-Melt transparent glaze
A base fluid-melt glaze recipe developed by Tony Hansen. With colorant additions it forms reactive melts that variegate and run. It is more resistant to crazing than others.
URLs https://en.wikipedia.org/wiki/Surfactant
Surfactants at Wikipedia
URLs https://www.zschimmer-schwarz.com/en/ceramic-auxiliaries/tiles/glaze-additives/wetting-agents
Wetting agents from zschimmer-schwarz.com: Surfactants that reduce the surface tension of aqueous glaze systems.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy