The chemistry of ceramic glazes are normally expressed as formulas. A unity formula has been retotaled to make the numbers of flux oxides total one.
Key phrases linking here: unity molecular formula, unity formulas, unity formula, umf - Learn more
A "unity molecular formula" (or UMF) is just an oxide molecular formula that has been retotaled so that the RO group of oxides sums to 1. It is a standard that provides one basis for comparing glazes. The three-column format of expressing a UMF was first used by Hermann Seger. Here is how we would recalculate a raw formula to a flux unity:
Raw Unity Oxides Formula Formula ----------------------------------- K2O 0.6 / 2.2 = 0.27 CaO 1.3 / 2.2 = 0.59 MgO 0.2 / 2.2 = 0.09 ZnO 0.1 / 2.2 = 0.05 ----- ---- Flux Total 2.2 1.0 Al2O3 0.9 / 2.2 = 0.41 SiO2 9.0 / 2.2 = 4.09 -----------------------------------
The Seger method of rationalizing the chemistry of glazes does not work as well at lower temperatures because some oxides that are powerful fluxes at high temperatures are refractory or inactive in low fire. Oxides have a much more individual presence or depend on interactions (at each temperature range) than the Seger method tends to recognize. Also, their contributions to particular properties often are not linear according to concentration. For example, boron is both a glass and a flux and the logic for its employment at various temperature ranges differs. It does not 'plug into' a Seger formula well. Many people prefer to use Mole% when rationalizing how a formula relates to the fired product. However, all of this being said, there is great value in a method of presentation that clearly shows the relationship between Al2O3, SiO2 and everything else.
Some argue that the UMF method of presenting glazes is not precise enough for glaze chemistry calculations. However, a greater source of imprecision is the accuracy of the percentage chemical analyses of the materials being used. Any method that calculates an exact match for an existing chemistry will also produce an exact match in UMFs. They work better for targeting when doing batch-to-chemistry calculations because additions or changes in the percentage of a material do not always change every number in the formula. However, it must be remembered that glaze chemistry is not about precise mathematics; it is comparative and best viewed in context and as a tool to help when comparing one thing with another.
Digitalfire desktop Insight required that users specify whether to unify recipes to RO or R2O3. However, Insight-live automatically sets this (the group having the greater total wins the unity setting). Users can click the 'Auto Unity' heading and it will cycle between various settings, eventually coming back to auto-unity. Recipes remember their settings.

This picture has its own page with more detail, click here to see it.
Ceramic material powders can be crystalline or amorphous (or a combination), and they can be natural or man-made, and they can have very different particle physics. Ceramic materials are classic case studies of the sciences of solid state physics and solid state chemistry. Mineral sources of oxides impose their own melting patterns in glazes. When oxides are then supplied by a different material, a new "system" is entered. An extreme example of this is sourcing Al2O3 to a glaze using calcined alumina instead of kaolin. Although the chemical formula of the glaze, as a whole, may remain unchanged, the fired result would be completely different. This is because very little of the alumina would dissolve into the glaze melt. At the opposite extreme, a different frit could be used to supply a set of oxides (while maintaining the overall chemistry of the glaze), and the fired result would be much more chemically predictable. Why? Because they readily release their oxides to the melt.
| Glossary |
Mole%
Mole% is a way of expressing the oxide formula of a fired glaze or glass. It is a preferred over the formula by many technicians who use glaze or glass chemistry. |
| Glossary |
Chemical Analysis
In ceramics, raw material chemistry is expressed a chemical analyses. This is in contrast to fired glaze chemistries which are expressed as oxide formulas. |
| Glossary |
LOI
Loss on Ignition is a number that appears on data sheets test results of ceramic materials and bodies. It refers to the amount of weight lost as it decomposes to release water vapor and various gases during firing. |
| Glossary |
Oxide Molecular Formula
In ceramics, the chemistry of fired glazes is expressed as an oxide formula. It expresses the relative molar proportions of the oxides contributed by a glaze recipe. There are direct links between the oxide chemistry and the fired physical properties. |
| Glossary |
Glaze Chemistry
Glaze chemistry is the study of how the oxide chemistry of glazes relate to the way they fire. It accounts for color, surface, hardness, texture, melting temperature, thermal expansion, etc. |
| Articles |
Converting between Oxide Weight %, Mole % and Unity Formula
Part of changing your viewpoint of glazes, from a collection of materials to a collection of oxides, is learning what a formula and analysis are, how conversion between the two is done and how unity and LOI impact this. |
| Articles |
How desktop INSIGHT Deals With Unity, LOI and Formula Weight
INSIGHT enables you to enter material analyses as recipes. This is a first step to inserting them into the materials database. Imposing an LOI and understanding how to set unity, and its connection with formula weight are important concepts. |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk