0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Case Mold | Casting Rate | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition During Ceramic Firing | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | DTA Test | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | LAS Body | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | LOI-Adjust | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Interaction | Oxide Molecular Formula | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | TGA Test | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Molecular Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Restaurant Ware

If you are a potter and want to make restaurant ware, read this. Many of the things you already think you know will mislead you in this type of venture.

Key phrases linking here: restaurant ware - Learn more

Details

Ceramics (mostly plates, cups, saucers) used in restaurants has, as its most important properties durability. The experience of trying to break a piece of this type of ware helps one appreciate how incredibly strong it can be. Restaurant ware is also easy-to-clean, non-leachable and has defect-free surfaces. Durable means that ware not only withstands rough handling but also sudden temperature change. And it does not scratch or cutlery mark. All possible clay surfaces are covered with glaze leaving only a foot-ring exposed. The body is dense enough not to absorb water where exposed. The glaze surface of leach-resistant ware does not dull on exposure to thousands of wash cycles. Restaurant ware is also also of consistent size and shape, it stacks and fits into dish washers well.

To be non-leachable and resistant to cutlery marking means that the suite of suitable pottery glazes you might have is much reduced. Common pottery glazes are often just too finicky for consistent results. Surfaces are often too matte and stain easily. Colored glazes often do not withstand the caustic environment in a dish washer. Just because a jar of commercial glaze says it is "food safe" does not mean it is "restaurant safe". This is not to say that only glossy glazes are suitable. While many matte glazes used in pottery stain easily and craze, it is quite possible to make very durable silky matte surfaces (examples are the G2934Y and G2571A recipes).

Using stoneware or porcelain, or firing to cone 6 or 10, does not automatically mean that you are making ware suitable for a restaurant. These terms have a different meaning in the pottery community than they do in a restaurant. In restaurants, "stoneware" is ware that is as strong as a stone. Potters think white-firing ware is porcelain, restaurants see it as white firing stoneware. The term "vitrification" is a process in pottery, "vitrified" is a term people see on webpages, there is generally no data to back it up. But a dishwasher in a restaurant can tell you immediately which ware is really vitrified.

If you want to make truly durable ware, an important tool you will need is a hammer. Break ware at every opportunity. And pay attention to what it does in comparison to commercial products. When ware breaks easily, be suspicious about how vitrified it really is. We do an SHAB test on all clays to get a picture of their density across a range of firing temperatures. And learn how to do the IWCT test (or something similar). Glazes must fit, with no tendency to craze or shiver. If they are under too much compression or tension, even vitreous ware will be weak and break-prone.

While durable ware can be made at lower temperatures, typically potters to not have the technical know how for this. It is best to fire higher and get the built-in benefits (easier glaze fit, glazes of higher SiO2 and Al2O3, bodies with a well developed mullite matrix). It is also best to employ a limited suite of base glazes, known to be balanced and durable. Add your colors, opacifiers and variegators to these. When other glazes catch your eye, identify the mechanism of their appearances and transplant that into your own base glazes.

Durable ware has smooth contours (no abrupt angles). Wall thickness are even across the pieces. Ware is dried and fired evenly so as not to build in stresses. Lips are rounded and not too thin.

Developing durable ware takes time. Slow evolution of firing techniques, glaze composition and application, body makeup and fabrication methods. You do not need fancy equipment. Strong and durable ware can be developed by anyone willing to do simple testing and development, by people willing to question what they are told, do the testing and get meaningful data. While some art can be a part of it, it is much more about craft and technical issues. Automation is your friend, because it can help maintain consistency, that is a big part of durability. And automation enables you to step back a little from personal involvement in the "art" to assess the "craft". Jiggering plates, for example, not only creates a more even cross section, but the increased production makes you more willing to smash a few to see how strong they are! And to think about vitrification and durability instead of just artistic merit. Casting mugs (instead of throwing) enables you to make your own clay body much more easily, a body you can learn to understand and tweak over time to improve it.

3D printing can also be your friend to make restaurant ware. It encourages you to carefully catalog cross sections of ware, classify them, develop them to work well together and be easier to make. 3D printing also makes it much easier to make molds, templates, tools and other things that aid production.

Related Information

Vitrification can be obvious by simple visual inspection


This picture has its own page with more detail, click here to see it.

The unglazed surface of the left piece has a sheen; it is a product of glass development during firing to cone 6. That body is a 50:50 mix of a cone 8 stoneware and a low-fire earthenware red (a material that would normally be melted by this temperature). Together they produce this dense, almost zero-porosity (zero water absorption) ceramic. The unglazed surface on the right looks more like plaster, and it is absorbent, about 5% porosity. It is a mix of the same stoneware but with 50% ball clay. The refractory ball clay ensures that the stoneware, which was already inadequately vitreous, is even more so. As you can imagine, the left piece is far stronger.

This super-vitrified clay bodies does this when fired


A super vitreous clay body

This picture has its own page with more detail, click here to see it.

Although not clearly visible in this photo, the unglazed body surface on both of these MNP (Plainsman 3D + 10% feldspar) pieces has a sheen - because they are super-vitreous. And broken surfaces appear like glass (as can be seen in the broken chips on the right). Because the foot-ring of the piece on the right is too angular it is plucking all the way around. This is not happening on the piece on the left for two reasons: The angle was rounded and it was fired on silica sand. Because it is so fine-grained (wet screen to 325 mesh) and contaminant-free the body tolerates firing well past the point of vitrification - not only resisting bloating and warping but giving something else: Incredible fired strength.

Smash Pots to Make Better Ones!

Learn their dirty little secrets.


Breaking pottery to learn about its quality

This picture has its own page with more detail, click here to see it.

One dirty secret that a fracturing piece can tell you is: "I am weak, easily broken". I just filled two five-gallon pails and three boxes (I use a nylon hammer, and safety glasses, of course). Every type of clay and glaze I use. Every temperature. I started with a commercial Denby stoneware piece to get a feel for how quality ware should break. It becomes immediately evident which pieces are weak by the way they shatter (and how high a strength-bar commercial ware sets). Breaks with knife-like edges indicate strong body/glaze combos. Strong ware breaks into fewer pieces. Crazed ware is really weak. Ware with glaze compression (even if not shivering) explodes on impact. Low-fire ware can be very strong when glazes fit (and even better when it is fired to cone 03 or 02). High-fire ware can be surprisingly weak (if not vitreous or glaze fit is poor). This is an example where individual potters can take responsibility for ware quality and learn when to avoid DIFM thinking.

Cone 6 whiteware vs. vitreous porcelain when it breaks


This picture has its own page with more detail, click here to see it.

The porcelain on the right (Plainsman Polar Ice), breaks much more like glass, to razor-sharp knife edges. But it is not a glass; it is a zero-porosity (no water absorption measured), dense matrix of glass-bonded crystals. The whiteware on the left (Plainsman M370) has 1% porosity, and although vitreous and quite strong, clearly it is not in the same class as the one on the right.

To gauge strength: Break pieces often. Pay attention to what happens.


A broken slip cast cone 6 mug

This picture has its own page with more detail, click here to see it.

This is M340 casting, L3798H. The handle was just glued on with slip. I had questions about this new body. Are my glazes under compression? How well is the handle stuck on? Because I have broken so many pieces I know how their fracture pattern. It is a good sign when there are no fractures along the handle joins. And when the handle is the last to go. And when the item breaks into large pieces rather than shattering into small ones. Try doing this on some of your pieces and you might be surprised. Either by how strong they are. Or by how easily they break.

Links

Glossary Fired Strength
Ceramics, by their brittle nature, have high compressive strength and unsurpassed surface hardness. Maximum fired strength can come at the expense of various working and fired properties, so testing is needed to reach a balance.
Glossary Leaching
Ceramic glazes can leach heavy metals into food and drink. This subject is not complex, there are many things anyone can do to deal with this issue
Glossary Cutlery Marking
Ceramic glazes that mark from cutlery are either not properly melted (lack flux), melted too much (lacking SiO2 and Al2O3), or have a micro-abrasive surface that abrades metal from cutlery.
Glossary Glaze fit
In ceramics, glaze fit refers to the thermal expansion compatibility between glaze and clay body. When the fit is not good the glaze forms a crack pattern or flakes off on contours.
Articles Concentrate on One Good Glaze
It is better to understand and have control of one good base glaze than be at the mercy of dozens of imported recipes that do not work. There is a lot more to being a good glaze than fired appearance.
Projects 2019 Jiggering-Casting Project of Medalta 66 Mug
My project to reproduce a mug made by Medalta Potteries more than 50 years ago. I cast the body and handle, jigger the rim and then attach the handle. 3D printing made this all possible.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy