0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Rate | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition During Ceramic Firing | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | DTA Test | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | LAS Body | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | LOI-Adjust | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Interaction | Oxide Molecular Formula | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | TGA Test | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Molecular Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Pour Spout

Plaster molds intended for slip casting have a spare at the top to act as a reservoir. This enables overfilling the mold to accommodate the dropping slurry level. 3D-printed spouts make a spare unnecessary.

Key phrases linking here: pouring spout, pour spouts, pour spout - Learn more

Details

Two handle mold styles: With and without a spare
The "spares" (in the slip casting mold on the left) act as built-in reservoirs to hold the extra slip needed (because of volume reduction during the casting process). These are the traditional way of making molds. However CAD and 3D printing enables rethinking this. The two 3D-printed pour spouts (top) glue onto the assembled mold on the right.

3D-printed pour spouts make it possible to create plaster molds that do not have a spare. Making these yourself is a great first step into getting into 3D design and 3D printing. Ideally, of course, you are also making your own spareless molds to work with them. Please do not overestimate the difficulty or underestimate the value of this.

The spare at the top of typical molds acts as a reservoir permitting overfilling - this accommodates the dropping slurry level as the mold pulls water. Although a traditional mold maker might consider the concept of a spareless mold ridiculous, 3D printing makes it not only more convenient, it just works better for many types of molds.

Related Information

Why 3D design and printing is a better way to make slip casting molds


3D printed plaster mold master

This picture has its own page with more detail, click here to see it.

I dread the traditional mold making process, the mess, all the supplies and tools involved. I am a potter, I make functional ceramics. I am not a mold-maker, but 3D design and printing have put it within my reach. This way more fun! There is no stopping this, it’s the future.
-I spend most time on design, pouring the plaster or rubber takes minutes.
-Many fewer tools and supplies are needed, the process is less messy, as easy as downloading a file, printing it and pouring in plaster - this is doable in my kitchen! I don't even need mold soap!
-Sanding of flat mating faces is possible (for better seams than I've ever had). This is because natches can be added later (using embeds).
-I can make my own natches and interlock schemes.
-No spare is needed, the 3D-printed pour spouts work better.
-The range of shapes seems limitless. Especially because designs can be split up into pieces, each printed in optimal orientation (and glued together).
-I make molds through multiple design-print iterations. 3D makes do-overs or changes in design as easy as a reprint and plaster-pour. So, I can make a mold just to test an idea!

A 3D-printed pour spout on a mug jigger-casting mold


3D-printed pour spout on a mug cast-jigger mold

This picture has its own page with more detail, click here to see it.

I prepare to attach these by simply touching them to the top of the slip (it is sticky and coats the underside evenly). Then it is just a matter of setting it in place and and it glues down in seconds. I make these a little larger diameter than the top of the opening in the plaster mold (e.g. 2mm), producing a small overhang on the cast piece (this one has 0.8mm thick walls and prints quickly). During the time in the mold, the clay slurry creates a thickness against the plaster walls that also extends upward above the top (inside the spout). Shortly after pour-out I put these into the cuphead on the jigger wheel and make a cut and lift the spout away. This leaves an over-hang and over-height that enable finishing the rim using the jigger template.

Slip cast calciner after pour out


This picture has its own page with more detail, click here to see it.

Pouring was made possible using a 3D-printed PLA pour spout. This enables overfilling the mold. The overhang lip is still optional, it was not possible to dry them enough to remove them from the mold without cracks appearing under the overhand (although if the mold is laid down as soon as possible after pouring this could work). Later we modified the spout to be flush with the inner wall and taller. And we added a drain hole so that pour out was not necessary - the spout thus just acts as a reservoir. Shortly after pour out we were able to remove it and cut the wall flush with the top edge. This enabled the clay to pull away from the mold with equal resistance all the way around, resulting in amazingly straight-walled pieces. And very thin walls were also possible.

A 3D-printed spout enables a flared rim on cast ware


This picture has its own page with more detail, click here to see it.

It was glued down using the casting slip itself (it stuck in seconds). About ten minutes after draining a fettling knife was run around the inside, then it detached easily. The overhung lip produced imparts structural strength that resists warping, for drying and firing, to the thin walled piece. This spout has advantages over the traditional "spare" built in to the upper part of a mold. It enables a one-piece mold. The lip can be more overhung. Draining is cleaner and easier. Molds are lighter. Extraction can be done sooner and it is easier. The spout does not absorb so there is less scrap. The degree of overhang is adjustable by simply printing new spouts.

Extreme example of 3D printed mold spouts


This picture has its own page with more detail, click here to see it.

These 3D printed mold spouts have been designed to perfectly fit onto this handle mold (they glue on with slip). On pour-out they can be removed and enable precisely cutting the join surface. The spouts are cleaned by allowing them to dry and throwing them into a bucket of water (the clay slakes off).

An impossible spout is possible by 3D printing


3D printed mold spout

This picture has its own page with more detail, click here to see it.

This mold is for a Medalta Potteries ball pitcher having a closed top with a teardrop-shaped spout (lower right). 3D printing makes it possible to create a pour spout that inserts perfectly into the angled hole, thus the plaster mold itself does not need a spare. The size of the pour spout reservoir and the degree of insert can tuned so that when the level drops to the bottom it is ready to pour and the pour hole is perfectly formed.

Bottle calibration mold demos novel casting methods


Plaster molds held together without straps

This picture has its own page with more detail, click here to see it.

Three slip casting methods are examples of the flexibility potters have compared to manufacturers (especially for small molds like this).
1) 3D-printed locks are stuck on to hold the mold halves together. The casting slip itself adheres them. Dipping the flat surfaces and attaching them takes seconds. This method enables aligning halves accurately and then locking them into place.
2) The 3D-printed pouring spout is also attached using the slip (it also helps hold the mold halves together) and acts as a reservoir and pour-out indicator. Thus, this mold needs no spare.
3) There are no natches (the halves were poured into disposable 3D printed PLA masters - and mate perfectly and align easily).
These three factors simplify the mold design, reduce mold size, improve the fit of parts and simplify pouring, demolding and cleanup for this specific type of piece.

A 3D Printed Mold Spout

Better Than a Spare for Slip Casting

Available on the Downloads page


A plaster mold pout spout

This picture has its own page with more detail, click here to see it.

Glue one of these on top of your slip casting mold (using slip) and enjoy the many benefits. These are intended for people who make their own molds using the 3D printing techniques taught on this website. Among the advantages are the following:
-Less mess.
-Smaller, simpler molds (they don't need a spare).
-Overhung lips, more precise lips.
-Visible indication of casting progress.

Inbound Photo Links


Here is what happens when I underestimate slip pressure

Mug handle molds with and without spares
Two handle mold styles: With and without a spare

Links

URLs https://www.instagram.com/reel/DeeiXK_CRou
3-D printed spout being used to fill plaster moulds
Three years after I first proposed this, someone is now actively promoting the idea. But in this case, the moulds still have a spare.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy