Oct 22, 2026: We are working on protecting our servers against the PHP2Shell vulnerability recently discovered. Servers were upgraded ahead of schedule on Oct 21. This could cause some issues. Please contact us if you encounter any.

3DP | BSG | AIF | ABR | | BIN | ADV | AGT | PHY | ASR | uAz | ALM | ALS | E11 | JWK | ART | ARC | EBA | LAG | PBA | NFi | BLC | mQi | BIN | 62N | BIO | BSQ | CHP | BDT | BGD | BGP | BFR | Csu | DZc | BRK | HWi | SCS | MCB | SCB | ECS | CSP | OLC | CRE | CPM | CRS | STN | CST | LBS | TIL | C3D | CBM | CLM | ECM | CLO | SLR | CRT | CCT | CLT | GBG | CCO | CCN | CRP | d3S | CGS | OCS | DEC | DFT | TM2 | | Dux | DRP | DSP | ELE | ELT | MUE | SEU | EEE | MEQ | SCE | EQD | EQP | EQM | EMR | SER | EQS | | ETC | P3D | PAR | PAU | PCA | PBF | PDE | PGL | PKB | PMM | PPO | PPP | PSH | PWT | EXT | FEL | TAA | FRC | 9h6 | FLB | kK5 | FLS | FRT | MFM | YtL | F3D | EGK | GNM | DGE | GBC | GBS | GLS | GLI | GLC | GLM | GLR | GLT | MGL | FGE | GLZ | GEQ | EHE | HMT | h79 | HTR | CHS | Niv | I3D | ICS | IDP | IGR | EAP | ISO | Qno | qhK | KAO | KCD | EKB | KIL | MKL | SKL | LNS | LAB | vLv | FRL | 7hb | LEM | CQL | LTR | MSH | MOF | MAN | | MRK | MDS | MMC | MPC | MTS | MTT | | MAM | MAA | MDE | MTE | EMP | MPE | CLM | DEN | PWH | MAT | e38 | MTR | BDW | PMF | MIN | 3MM | MMK | EMM | MNC | EMF | yPu | NOX | SOC | | DSL | OPA | QKk | OXI | RED | PTT | SWS | PPS | PNC | PRP | | SPM | SPB | MPB | FRP | 9Hv | POI | PEN | PTW | PEQ | a87 | WKS | EPR | PRS | PRT | | PRD | PRO | | | | QCC | RMP | RSR | SRM | MRM | MGR | RFR | wWm | REF | SRS | EAR | ESK | SWR | | SCU | | YFh | SIL | ESR | LrD | YnJ | ESP | MSM | Tmx | STC | OLS | k67 | JXh | PWS | TWC | EPW | TCP | TCE | WSN | TLS | MTL | STL | TGR | OTR | | | UNI | UVR | FWK | gLF | WRS | WPS | YQd

Glaze Chemistry

Case studies where glaze chemistry was used to solve a problem.

Related Information

A high feldspar glaze is settling, running and crazing. What to do?


Blue glaze with chemistry calculations

This picture has its own page with more detail, click here to see it.

The original cone 6 recipe, WCB, fires to a beautiful brilliant deep blue green (shown in column 2 of this Insight-live screen-shot). But it is crazing and settling badly in the bucket. The crazing is because of high KNaO (potassium and sodium from the high feldspar). The settling is because there is almost no clay in the recipe. Adjustment 1 (column 3 in the picture) eliminates the feldspar and sources Al2O3 from kaolin and KNaO from Frit 3110 (preserving the glaze's chemistry). To make that happen the amounts of other materials had to be juggled. But the fired test revealed that this one, although very similar, is melting more (because the frit releases its oxides more readily than feldspar). Adjustment 2 (column 4) proposes a 10-part silica addition. SiO2 is the glass former, the more a glaze will accept without losing the intended visual character, the better. The result is less running and more durability and resistance to leaching.

Is the N505 cone 6 matte glaze recipe what you think it is?


N505 pottery glaze

This picture has its own page with more detail, click here to see it.

This recipe is from page 2 of the booklet: "15 Tried & True Cone 6 Glaze Recipes". Click the following code, G3955, to see more information on how it compares with G2934 and G1214Z1 mattes. This flow test and these test tiles were in the same kiln, fired at cone 6 using our PLC6DS schedule. The defining characteristic of N505 is its extreme melt fluidity - it runs because it is overtired at cone 6. Still, the surface on the tile (lower right) is arguably more interesting than G2934. Some felt pen marking reveals why: The micro surface is much rougher. To its credit, although it does stain easier, it can still be cleaned with effort.

From the chemistry, shown on Insight-Live side-by-side screenshot. It has very low Al2O3 and SiO2 - that turns on some red and yellow lights. One could hope to have melt fluidity and great functionality, but they pretty well never go together. This glaze should fire glossy - the 6% magnesium carbonate is the mechanism of the matteness - MagCarb is super refractory, it may not be dissolving in the. melt. The glaze should cutlery mark (although it seemed hard in our testing). Most important, low Si:Al levels always carry the risk of leaching - exercise caution adding any significant percentage of heavy metal pigments. Crazing is another possible issue over melted glaze.

Li2O from Spodumene instead of Lithium Carbonate:

Good chemistry and economy, but bad physics


Two very melt fluid glazes

This picture has its own page with more detail, click here to see it.

Lithium carbonate is now ultra-expensive. Yet the reactive glaze on the left needs it. Spodumene has a high enough Li2O concentration to be a possible source here. It also has a complex chemistry, but the other oxides it contains are those common to glazes anyway. I did recipe rescue calculations and got a pretty good match in the formulas (lower section in the green boxes). Then I made 10-gram balls and did a GLFL test at 2200F.

Not surprisingly, this recipe is very runny; that's why the tiny yellow crystals grow during cooling. The new version fires very similarly, perhaps better. My calculated cost to mix these in 2022 was $17.84/kg vs. $10.40/kg. In 2026, the difference is even greater! But there is a practical cost: Poor slurry properties. The spodumene sources so much Al2O3 that 70% Alberta Slip had to be dropped to accommodate it! How does one use this type of glaze without ruining kiln shelves? Using a catcher glaze is one answer.

High feldspar glazes craze on functional:

Don't put up with it. Fix them.


This picture has its own page with more detail, click here to see it.

This glaze, "Bamboo Cone 10%", contains 50% potash feldspar, so it certainly qualifies as a high-feldspar glaze. K2O and Na2O are thus oversupplied. They have the highest thermal expansions of all oxides, by far. These are needed and valuable, but when grossly oversupplied the result is crazing. This glaze used to work on this body, H550. The previous version of H550 was firing near the bloating point of the body, about 1% porosity, so the recipe had to be changed to provide more margin for error. The new recipe has a more practical 2.0-2.5% porosity; it has no danger of bloating or warping and still has excellent maturity and strength. This glaze was crazing before, and pieces did not leak because the body was dense enough - so they were still watertight. But now it does not work. The solution is to do something that should have been done before: Use a silky matte base recipe that does not craze. I recommend the G2571A base (below right) - the Zircopax, rutile, and iron oxide in the original can be added to it instead.

Cone 10R clear glaze made more "clear":

Using frit to source Na2O instead of feldspar


Side-by-side melt flow test samples

This picture has its own page with more detail, click here to see it.

To get a better, more brilliant transparency than G1947U, at cone 10R, I tried sourcing Na2O from a frit. The inside surface on this mug is the result (v2), it is so glossy it looks like a low-fire leaded glaze. This screenshot of side-by-side panels shows the frit-enhanced version(s), G3910 and G3910A. Frit 3110 has a much higher concentration of KNaO than the feldspar, a key to making a brilliant glass. While this increases the COE, the fact that it comes from this frit brings multiple benefits:

-A brings a little B2O3, a better melter than zinc (which volatilizes anyway at cone 10).
-It dissolves more low-expansion glass-forming SiO2 (in v2 I switched to 400 mesh silica to enhance that even more).
-The glaze can then tolerate some low-expansion MgO (introduced by Frit 3249 or its equivalent, Fusion Frit F-69).

More details about this project can be found by clicking/tapping the Insight-live recipe code numbers G1947U, G3910 or G3910A. The red outside glaze is G2571D1.

Sanity checking a cone 6 purple pottery glaze


A purple pottery glaze that shivers

This picture has its own page with more detail, click here to see it.

A customer was having serious trouble with this cone 6 glaze recipe shivering. A quick check of its chemistry reveals the reason: It has the lowest calculated thermal expansion we have ever seen! The reason is the high spodumene and talc levels. Adding the 3% cobalt also makes this among the most expensive we have seen. To say this recipe looks non-typical is an understatement. And, it raises flags on working properties and susceptibility to leaching in both limit recipes (e.g. very low clay content, high talc and spodumene) and limit formulas (stratospheric levels of Li2O and MgO coupled with plenty of cobalt).

The hard panning problem can be fixed easily: Supply the same amount of Li2O from lithium carbonate (only 10% is needed so the overall recipe cost is reduced), which makes room in the recipe for clay (to supply the lost Al2O3 and SiO2 from the spodumene). Second, introduce KNaO at the expense of MgO and Li2O, which will greatly increase the thermal expansion and reduce or stop the shivering.

Use a frit blend ratio to control the amount of kaolin in a glaze recipe


Side-by-side recipe screenshot

This picture has its own page with more detail, click here to see it.

These are the recipes and calculated oxide chemistries of two pottery glazes (as shown in my account at insight-live.com): The original problem recipe and an adjustment to fix it. Recipe #1 sources boron from a soluble material and three plastic materials are combined to increase drying shrinkage enough to cause cracking when drying (and thus crawling). Recipe #2 solves these problems while producing the same chemistry. It sources boron from two frits (one having almost no Al2O3) whose ratio to each other can be altered to supply more or less Al2O3 to the melt. That enables removing two of the plastics: Ball clay and Gerstley Borate. The remaining 20% EPK is perfect to create a creamy slurry that suspends, applies and dries well.

Imagine realizing that pottery you're selling is all going to craze!


A glaze is crazing. Here is why.

This picture has its own page with more detail, click here to see it.

What if every single piece you have been making is all eventually going to craze? Do you refund all the customers? All because you trusted a liner glaze recipe found online. At a reputable site. This recipe is called "Classic White". And it has "classic crazing". On going back to the source web page you find there is no mention of even the possibility of crazing. Then you type the recipe into your account at Insight-live.com and are horrified to see how high the thermal expansion calculates to (see red circles on picture). Then you realize that, based on simple recipe limits, you could have steered clear of this just by looking at it. Then you find there are other well-documented base glossy and matte recipes that do not craze (like G2934 and G2926B). Even if they do they are adjustable to enable fixing the issue. And you can even blend them to create any degree of satin desired. And they use a mix of tin oxide and Zircopax to avoid crawling. And they are durable, don't cutlery mark, don't leach, don't run, don't settle in the bucket.

Substitute Ferro Frit 3134, using glaze chemistry, in three glaze types


Insight-live screen shot, substituting frit 3134

This picture has its own page with more detail, click here to see it.

Can't get frit 3134 for glaze recipes? Can you replace it with frit 3124? No, 3124 has five times the amount of Al2O3 (the second most important oxide in glazes) and half the amount of B2O3 (the main melter). This ten-minute video presents a glaze chemistry approach that is easier to do than you probably think. It deals with three different glaze recipe types lacking sufficient clay to suspend the slurry. Learn to source the needed oxides from two other Ferro frits, 3110 (or Fusion F-75) and 3195 (Fusion F-2), and end up with at least 15% kaolin in each. A unique approach is required in each situation. Two of the calculations produce improved slurry properties and one yields a recipe of significantly lower cost. If you have a recipe that needs this and need help please contact us.

This pottery glaze is peeling when multi-layered:

The recipe reveals why.


Pottery glaze peeling

This picture has its own page with more detail, click here to see it.

Dipping glazes can, in very controlled circumstances, be multi-layered. If you have done it for some time, with success, you may have been just lucky. These pieces demonstrate one of many factors that can produce failure: The top glaze contains 7% bentonite and 5% zinc oxide - that is 12% hyper-fine particles, perfect to create the drying shrinkage to make this happen. The recipe author must have reasoned that it could "pinch hit" for the inadequate clay content. But 7% bentonite in any glaze is highly unusual. And, it is actually not even necessary here. Why? The high percentage of Ferro Frit 3124 is sourcing needless Al2O3 (alumina), that should be coming from kaolin or ball clay instead. Frit 3134 is the perfect stand-in, it contains almost no Al2O3, but otherwise is quite similar. The equivalent recipe we calculated on the right has the same chemistry, but does pass a sanity check. It is not guaranteed to work, but has a better chance than this one. For even more assurance of success, it should be mixed as a base-coat dipping glaze.

Lithium carbonate and Gerstley Borate in glazes:

What is the best way forward?


Four common lithium carbonate glazes

This picture has its own page with more detail, click here to see it.

Lithium is getting really expensive. These are four recipes submitted by a customer who wonders if there is a substitute. The answer is not simple; each glaze is a unique situation. Fortunately, lithium carbonate is almost always a minor addition (in the first two recipes it is 1% and 3%). Lithium is a powerful low-expansion flux; in some cases, a low-melting, low-expansion frit could perform the same function (e.g. Ferro 3249). Even for the 6.5%, as in the third one, this could still work. But in these cases, wouldn't it be better to continue using lithium? Even for the last one that has 9%? It's only expensive if you make glazes and don't use them. Perhaps a solution is to make them as brushing glazes; a 1-pint jar only needs about 350g of powder (that is only about 30g for recipe 4).

This situation can also be considered an opportunity to rationalize the recipes you use. Let's pretend that each of these might be used on functional ware and should measure up to common-sense recipe limits. The Gerstley Borate in three of these is also a red flag; it won't be available shortly (calculating how to source B2O3 from frits is better anyway). During that process, you might find that lithium is not even needed. Another issue is thermal expansion. Notice that one of these calculates to 8.5 and another to 9.6! Those are virtually certain to craze. Why not lower that number while removing the Gerstley Borate? Notice that two of these have clay percentages over 70% (Alberta Slip and Gerstley Borate), these are virtually certain to crack on drying (and crawl on firing), that can also be fixed. The percentage of titanium, Zircopax and rutile in the fourth one are highly likely to make it crystallize heavily on cooling produce problems with cutlery marking and staining.

From Scribbles to Success: Fixing This Glaze Recipe


Pottery glaze recipe scribbled onto a card

This picture has its own page with more detail, click here to see it.

If you do DIY pottery glazing you may have recipes scribbled onto cards like this. But the card is not the big issue here; it is that recipe! It really needs some work. Here is what could be done.
-Add this as a recipe in an account at insight-live.com (and assign it a code number to write on all test specimens) to start a testing project. Along the way document it with pictures, firing schedules, general notes, etc.
-With all that feldspar, it is sure to craze, reducing the high thermal expansion K2O it contributes in favor of low expansion MgO (from talc) is the first fix to try.
-With all that clay (29 total) it is likely to crack while drying (and then crawl during firing). Try reducing shrinkage with 29 kaolin (no ball clay). If it still cracks, substitute some for calcined kaolin.
-And those colorants: It is better to use cobalt oxide than carbonate. A burnt umber increase could be tested to eliminate the need for both the manganese and iron (since it supplies both and has zero LOI). Better yet, remove all four and use a black stain (7% would likely be enough).
-Perhaps the best option is to get a different glaze recipe. This is a calcium matte to G1214Z1 would be a good start. For a more pleasant surface, G2934.

Max out a native clay in a new glaze recipe:

Turning Plainsman 3B into a transparent base glaze


This picture has its own page with more detail, click here to see it.

A screenshot comparing the chemistries of two recipes. The recipes are different, but the chemistries are the same. On the left, Plainsman 3B (also known as MNP) is being used to source almost all of the Al2O3 (the red box) needed by the recipe (to match our standard cone 10R transparent G1947U, on the right). The KNaO is being sourced from the frit rather than feldspar (this is really good because it has almost no Al2O3, so all of it can be sourced from the 3B clay). Only silica and calcium carbonate are needed to bring the SiO2 and CaO up to match the glaze being used as a pattern.

Frit vs Feldspar in a cone 10 glaze:

A good reason to do that.


Side by side melt flow tests of the original glaze and the fritted variation

This picture has its own page with more detail, click here to see it.

I calculated a frit-based recipe to match the original G1947U Cone 10R clear feldspar-based one. Only after seeing the fired results did I fully realize how much better it melts and how much more transparent it fires. It costs more money to make, but in some situations it is worth it.

My original approach was just theoretical: Shift KNaO-sourcing from feldspar to frit to get a better melt. As calculations took shape, it became clear that I could increase KNaO because it enabled increasing SiO2 also. When the kiln opened, I got a surprise with the original G1947U: It never looked white on the ware, but when seeing it thick like on this GBMF test (bottom), it looks really cloudy. Likely the melt is not completely dissolving the particles of quartz! The surface brilliance of the new G3910 blew me away at first; it really is better (top right is G1947U left, G3910 right on buff and brown bodies). This glaze develops a better interface with the body and on porcelains, it is more crystal clear and much brighter.

Glaze calculation in the 1960s


This picture has its own page with more detail, click here to see it.

This batch-to-formula calculation was done by Albert E. Holthaus at Modern Art Products Company in Kansas City, MO (during the 1960s). Doing this not only seems quaint today, but suppliers put up roadblocks to doing it.

Notice that he took the manufacturer-supplied percentage analysis for each material (bottom) and calculated the unity formula for use in his batch to formula calculation (top). The recipe material weight amounts are missing in the latter; this appears to be his effort to create a documentation page of the recipe on the oxide formula level (this is what mattered to him). It was a time when frit formulas were published by their manufacturers. He also calculated the glaze's chemistry as a percentage analysis, likely to lay a basis to assess it against stated requirements from stain suppliers (certain stains only work when the host glaze chemistry meets a certain profile).

Doing this now is so much simpler. But almost no one actually does! The closest most technicians get to oxide formulas is choosing a frit from a list of ones for which the chemistry given by the manufacturer is only approximate.

Ferro Frit 3134 is NOT A SUBSTITUTE for Gerstley Borate


Gerstley Borate vs Frit 3134

This picture has its own page with more detail, click here to see it.

This frit, or any of similar chemistry (e.g. Fusion F-12) IS NOT A 1:1 SUBSTITUTE for Gerstley Borate, their chemistries are too different. That being said, the frit sources lots of B2O3, which makes it a candidate to weave into recipes as the source of boron. To show the difference, I have put 100 parts of each in side-by-side recipes in my Insight-live.com account, set the calculation type to non-unity formula and increased the frit until the B2O3 in the two match. Notice it takes 118g of the frit to source the same amount of B2O3 as 100 GB. Notice also that the frit sources almost triple the amount of Na2O per weight unit (that is a big deal because it means the recipe containing the Gerstley Borate to be substituted needs an Na2O-sourcing material that can be reduced to compensate). And the frit sources 3.5 times the SiO2 (other SiO2-sourcing materials in the recipe will need to be cut to compensate). And the Gerstley Borate has significant MgO while the frit has none (so an MgO-sourcing material like talc will be needed). Minor tweaks will also be needed to reduce other sources of CaO (since the frit has quite a bit more). The recipe will also need enough flexibility to do the final matching of Al2O3 and SiO2. The GBMF test confirms the difference at 1700F; these 10-gram balls melted down onto the tiles very differently.

A calcia matte glaze was leaching:

A potter fixed it with a simple formula change.


A potter fixes a leaching glaze

This picture has its own page with more detail, click here to see it.

G1214Z1 is a cone 6 calcia matte glaze, it has very high melt fluidity, enabling a fine-grained crystalline matte surface to develop during cooling. A potter was steered to this recipe after finding that G2934 magnesia matte fired too variegated when stained blue. However, this failed a leaching test. So, she simply increased the SiO2 in the formula (as shown in this Insight-live screenshot of doing the chemistry). SiO2 is the glass that makes up the lion's share of all glazes, but in mattes it is minimized in favor of Al2O3 (which often comes at a cost of susceptibility to leaching). The new recipe passed the GLLE test for leaching and even enabled reducing the cobalt percentage! Notice there is a cost: She had to compromise the degree of matteness somewhat to get the more durable product (the Si:Al ratio is a factor in the degree of matteness).

G2934 plus 10% silica actually flows more


This picture has its own page with more detail, click here to see it.

Until now, I thought magnesia matte glazes need high Al2O3 and a low Si:Al ratio. But this melt flow test suggests otherwise. The cone 6 glaze on the left (A) is close to my usual target of 0.4 MgO, 0.1 B2O3 and a ratio of 6:1 (approaching ceramic tile proportions). It is thus a classic high-MgO / higher-Al2O3 magnesia matte. The melt's high viscosity, limited flow, and phase separation produce the very fine surface texture.

However, glaze B has a super-high Si:Al ratio of 14:1. Yet it is not running much more and is almost as matte. How? It seems I shifted the matteness mechanism. Cutting the Al2​O3​ in half and spiking the SiO2​ has moved from a high-alumina magnesia matte toward a low-alumina, high-silica calcium/magnesium silicate matte. The massive surplus of SiO2 coupled with oversupplied MgO and plentiful CaO has weakened the "glue" that keeps the latter busy in the glass matrix, so they precipitate out (as calcium-magnesium silicates, diopside CaMgSi2​O6​ or enstatite MgSiO3, according to Google). This still creates a matte surface by crystallization and phase separation. The degree of matteness could likely be enhanced by slow cooling. And possibly 400 mesh silica.

Online Glaze Recipe Rescue:

Seeks good home for a magnesia matte blue


This picture has its own page with more detail, click here to see it.

This "Minty Matte" glaze was found wandering in a Facebook group. The current "home" is a base recipe having high nepheline syenite coupled with very low SiO2 (thus high COE). It crazes on most clay bodies used by the potter who contacted me. Its tag traced it to Glazy 20196. I sometimes think of these as "shelter recipes", needing a "glaze rescue". The beautiful appearance of this one provides the motivation to give it a little love and rehome it into a new base recipe! The love it needs is a simple understanding of the mechanism to move: It is rutile saturation in a magnesia matte with a little cobalt to kick the blue. Base recipes aren't carved in stone; the chemistry of this one can be altered to drop the COE a lot (by switching Na2O for MgO). G2934 magnesia matte also works with this mechanism (and has a much lower COE). Transplanting the rutile and cobalt into it would surely reduce crazing.

However, this recipe needs another rescue. From a misunderstanding. Although the potter contacting me was happy with the G2934 as a base for the rutile and cobalt, she had learned that durable glazes should have an R2O vs RO Ratio of around 0.3:0.7 (G2934 is 0.1:0.9). However, the R2O:RO ratio thing is misunderstood. Durability is much more about producing a well-melted homogeneous glass (but not over-fluid) with minimal phase separation and surface crystallization, good body fit and absence of large amounts of easily dissolved colorants.

A transparent glaze is going satin:

Is it the feldspar and kaolin substitutions?


Made on Gemini from the potter's description of the problem. AI Policy

This picture has its own page with more detail, click here to see it.

A potter reports that a switch from G-200 feldspar to Mahavir, and EPK to Imerys kaolin, has resulted in this transparent glaze becoming more satin. Is that possible? Yes. Because this glaze is on a unity formula tipping point.

To see it, you do not need to know how to do glaze chemistry, just how to display the calculated unity formulas side-by-side. My Insight-live shows them here. The material change has little effect. But there is an anomaly: 0.29 MgO. That is magnesia matte territory. The MgO is very likely there to help bring the thermal expansion as low as possible (to avoid crazing). For people who cool their kilns relatively quickly, this fires glossy. But a material change could well affect the cooling rate needed to maintain the gloss. That being said, the potter may also be firing slower, yet attributing the mattness to the materials. Or it could be a combination of both.

This is a popular glaze, among others in the book "Mastering Glazes". In Ron Roy's circumstances, and for many others, it is glossy. But for this potter, a small change (in the recipe materials and also likely in firing) has produced this issue.

Petalite for Lithium Carbonate:

It takes eight times as much!


This picture has its own page with more detail, click here to see it.

Here are the three common lithia source materials in a side-by-side calculation to compare their potencies. I have adjusted the material weights so that all are delivering the same amount of Li2O (assuming a recipe calling for 5% lithium carbonate).

By weight it takes 42 parts of petalite to deliver the same amount of Li2O as 5 parts lithium carbonate! But notice how much SiO2 and Al2O3 come along, major surgery on the host recipe is needed to compensate for this (if even possible). Spodumene is complicated too, it brings along so much Al2O3. That’s a problem because the most frequent existing Al2O3 supplier, clay, may have to be greatly reduced or even eliminated (producing a recipe that does not suspend in water). The other baggage both materials bring is lots of SiO2, especially petalite. Thus, replacing lithium carbonate with petalite or spodumene is not really a material substitution—it is a glaze reformulation.

An unfritted tile glaze is boiling and spattering the kiln shelf above


A boiling tile glaze spatters the shelf above

This picture has its own page with more detail, click here to see it.

This recipe is part of a project to reproduce chemistry previously achieved using Fusion Frit FZ-16. Glazes made with that frit do not exhibit this violent boiling and produce ultra-gloss surfaces comparable to those formerly obtained using lead frits. The likely culprit here is not simply the oxide chemistry, but the way it is being sourced: borax pentahydrate releases large amounts of water during heating and calcium carbonate releases CO2, while the borax is already helping to form an early borate-rich melt. The high ZnO likely influences the viscosity and surface tension of that melt, possibly making gas escape more violent. In the fritted version, much of this chemistry has already been reacted during frit manufacture, dramatically reducing gas evolution during the glaze firing.

This illustrates something broader than a weird glaze defect: you can duplicate an oxide formula without duplicating the way the glaze behaves on the way to becoming glass.

Lithium is no longer affordable for ceramics.

Yet in many cases it seems indispensable


This picture has its own page with more detail, click here to see it.

The crystals that form as this cone 6 fluid-melt glaze solidifies are one of the minerals in the recipe: Spodumene. Actually β-spodumene. But it is so expensive, and there is 42% here! What would it take to reduce the cost of making this glaze ($52/kg in 2026)? Another flux could certainly make it just as melt-fluid, but it would not grow spodumene crystals.

β-spodumene is Li2O - Al2O3 - 4SiO2 So the 0.22 Li2O in this glaze would require 0.22 Al2O3 and 0.88 SiO2 to crystallize as a β-spodumene-type lithium aluminosilicate. The glaze contains 0.24 Al2O3 and 1.41 SiO2. There is almost exactly enough lithium to combine with nearly all of the alumina as β-spodumene. The 2% rutile supplies TiO2; it acts as a nucleating agent. Replacing Li2O with another flux could maintain the melt fluidity, but Na2O, K2O or B2O3 cannot simply take the place of Li2O in β-spodumene.

It is possible that less spodumene could still do this. That could be tested by reducing Li2O to 0.1 and increasing Na2O to 0.23 (while maintaining the other oxides as-is). B2O3 could also be tried (it has a far lower thermal expansion). Of course, effecting changes in specific oxides requires some glaze chemistry.

Mastering Glazes High-Cal Matte crawling:

Know Tile #6 kaolin, know the fix.


This picture has its own page with more detail, click here to see it.

The kaolin is implicated in this glaze crawling problem. 30% EPK is a lot - a tipping point for issues with shrinkage and cracking on drying. Although #6 Tile kaolin in its place (center) doesn't disrupt the overall chemistry, it does disrupt the drying shrinkage: it is just too plastic for that high a percentage in a recipe. The fix is to substitute part of it for calcined kaolin.

Calcined kaolin has no LOI (vs 12% for raw kaolins). Without overthinking it, LOI-adjust by considering that 10% less is needed. So 20% #6 Tile and 9% calcined kaolin will equal 30% EPK. The right panel shows the calculated chemistry of the recipe with this change; notice it is very close to the same.

There are other fix options also. NZ and Grolleg kaolins are less plastic choices than #6 Tile; using either might mean that no calcined material is needed. Also, the failure happened on multi-layering of dipping glazes; crawling is common with that. The base glaze could have been mixed as a base-coat dipping glaze.

Same glaze chemistry, very different LOIs.

Look at the bubbles!


This picture has its own page with more detail, click here to see it.

These two GBMF test balls were melted on refractory tiles to compare their melting behaviour. Their calculated oxide chemistries are almost identical, but their recipes are very different. G2931F (left) contains 29% Ulexite, driving its calculated LOI to 14.3%. G2931K (right) sources its boron from frits, reducing the LOI to just 3.1%. The difference is striking! The high-LOI glaze is full of large bubbles that were unable to escape or clear before the melt stiffened during cooling. Although ulexite releases most of its chemically bound water before significant glaze melting, that early gas evolution can contribute to foaming and trapped bubbles as melting progresses. The fritted glaze is much clearer, although it still contains fine bubbles. These may be associated with the kaolin or other sources of entrained gas.

The GBMF test exaggerates gas-retention behaviour, which is precisely why it is useful for comparing recipes, but it does not necessarily predict the appearance of a thin glaze layer on ware.

Links

Video
How I Developed the G2926B Cone 6 Transparent Base Glaze
How I found a pottery glaze recipe on Facebook, substituted a frit for the Gerstley Borate (using glaze chemistry), compared using a melt flow tester, added as much extra SiO2 as it would tolerate, and got a durable and easy-to-use cone 6 clear.
Video
Converting G1214M Cone 6 transparent glaze to G1214Z matte
I converted a glossy transparent pottery glaze into a matte glaze using glaze chemistry and recipe logic. Watch me do it in my account at Insight-live.com. We'll cut the Si:Al ratio, increase the CaO further, maintain the thermal expansion for glaze fit and make the recipe shrinkage adjustable using a mix of calcined and raw kaolin. See the landing page to learn every detail: https://digitalfire.com/picture/3787.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved