3D Print a Test of the Beer Bottle Neck
3D Printing a Clay Cookie Cutter-Stamper
A 3-minute Mug with Plainsman Polar Ice
A Broken Glaze Meets Insight-Live and a Magic Material
Accessing Recipes from "Mid-Fire Glazes" book in Insight-Live
Adjusting the Thixotropy of an Engobe for Pottery
Analysing a Crazing, Cutlery-marking Glaze Using Insight-Live
Compare the Chemistry of Recipes Using Insight-Live
Connecting an External Image to Insight-Live Pictures
Converting G1214M Cone 6 transparent glaze to G1214Z matte
Create a Synthetic Feldspar in Insight-Live
Creating a Cone 6 Oil-Spot Overglaze Effect
Design a Triangular Pottery Plate Block Mold in Fusion 360
Designing a Jigger Mold for a Bowl Using Fusion 360 CAD
Downloading and 3D-Printing a 3MF file
Draw a propeller in Fusion 360 for use on an overhead propeller mixer
Drawing a Mug Handle Mold in Fusion 360
Drawing a Mug Mold Using OnShape CAD
Enter a Recipe Into Insight-live
Entering TestData Into Insight-Live
Fine tune the thixotropy of a glaze or engobe slurry
Getting frustrated Gerstley Borate turning glazes to jelly
How I Developed the G2926B Cone 6 Transparent Base Glaze
How I Formulated G2934 Cone 6 Silky MgO Matte Glaze Using Insight-Live
How to Apply a White Slip to Terra Cotta Ware
How to Paste a Recipe Into Insight-live
Importing Data into Insight-live
Importing Desktop Insight Recipes to Insight-live
Importing Generic CSV Recipe Data into Insight-Live
Insight-Live Meets a Silica Deprived Glaze Recipe
Insight-Live Quick Tour
Liner Glazing a Stoneware Mug
Make a precision plaster mold for slip casting using Fusion 360 and 3D Printing
Making ceramic glaze flow test balls
Making test bars for the SHAB, LDW and DFAC tests
Manually program your kiln or suffer glaze defects!
Mica and Feldspar Mine of MGK Minerals
Predicting Glaze Durability by Chemistry in Insight-Live
Preparing Pictures for Insight-live
Replace Lithium Carbonate With Lithium Frit Using Insight-Live
Replacing 10% Gerstley Borate in a clear glaze
Same Beer Bottle Mold Using Fusion 360 and OnShape CAD
Signing Up at Insight-live.com
Signing-In at Insight-live.com
Slip cast a stoneware beer bottle
Substitute Ferro Frit 3134 For Another Frit
Substituting Custer Feldspar in a Cone 10R glaze recipe
Thixotropy and How to Gel a Ceramic Glaze
Use Insight-live to substitute materials in a recipe
Watch Thixotropy Happen With a 20kg Batch of Dipping Glaze

How I Developed the G2926B Cone 6 Transparent Base Glaze

How I found a pottery glaze recipe on Facebook, substituted a frit for the Gerstley Borate (using glaze chemistry), compared using a melt flow tester, added as much extra SiO2 as it would tolerate, and got a durable and easy-to-use cone 6 clear.


Click here to watch this at youtube.com or click here to go to our Youtube channel

Transcript/Notes

1
Every potter needs a reliable transparent glaze that fits the studio clay bodies, works well with colorants and has good mixing and application properties.
I want to show you a different approach on how to do more than just try one new recipe after another.
Here is the first thing that’s different: Treat it as a project worthy of being in your permanent testing history. The best way to do that is in an account at insight-live.com. I’ll start by adding a new recipe. I already have the new one I want to try on the clipboard, so I'll click the "Import button”, paste it into the box, check "Confirm", then "Interpret".

more.. 2
Notice this material is not being found. That means it won't contribute to the calculated chemistry I am going to be doing shortly. In the Materials Manager I’ll search it in “Our Materials” (rather than the reference ones).
Notice that we have our own version of this material defined - this was done in order to include a cost. However it is still pointing to the reference one for the chemistry.
I'll click the blue edit button in the recipe panel and fix the spelling.
I'll also type in the name of the glaze.
One more thing to notice: I am not entering anything in the units column, this is only needed in special circumstances.

3
Here is the second thing I do that’s different: I assign it a code number: In this case "G2926A", it is the link between physical tests and their testing data. It gets written on every test sample and every container. Finally I save it by clicking “Done Editing”.

4
There is the third thing I do that is different: I sanity-check the recipe.
Notice this material: Gerstley borate (please forgive me for my pronunciation). This puts up an immediate flag, we'll learn more in a minute. This was a natural calcium borate mineral - actually, it was a "clay". Although complex chemically, the reason it was so popular is this oxide: B2O3 - this is boron. This oxide is the key enabler for glaze-melting at cone 6. If you need a reminder of why boron is so important, just click "here".
Back to the question here: Do I really want to use this material? Today the answer is "no" because it is no longer available. Yet you will find this in hundreds, perhaps thousands, of recipes. Years ago the answer was also no - but people endured all of its issues anyway, mostly it was because they didn't know the simple alternative we are about to use! If you would like to learn more, just click here.

5
There is the fourth thing I do that is different: I look at the chemistry.
Notice that, in addition to boron and minor amounts of other oxides this material sources significant calcia, magnesia, soda and silica. So, let’s replace it with a calcium borate frit - which also sources those other oxides.
To start, I’ll duplicate this recipe and click the blue edit button and name it "Studio Clear v2" with a code number of "G2926B".
I'll replace the material name with: “Ferro Frit 3134" and click "Done Editing".
Let’s open these two materials in side-by-side panels. The frit has a little less boron but the other oxides it delivers look familiar, although in quite different proportions.

6
Next, let's turn on chemistry calculation for the two recipes so we can compare them on the oxide level.
Let’s start with the boron, the yellow number. It is "down" in the new recipe, more frit is needed to supply enough.
While I could just repeatedly edit recipe amounts to zero in on the 0.33 target, there is a better way.
I'll start "calculation mode", set the increment to 2, and nudge up the frit amount until the boron matches.

7
Next, let's add a little talc to contribute the magnesia. I'll add a line, enter the name, an amount of one, and finish editing. I’ll change the “increment amount” to 0.5 and click its up-arrow until the MgO matches that in the chemistry of the original recipe.

8
Now, let's fine-tune the K-N-aO. Notice it is also supplied by the nepheleen syenite. I’ll reduce that, three at a time, until the oxide amount matches the 0.32 value of the original oxide formula.

9
Just a note that I have fixed an error here - the recipes should be code numbered G2926 and G2926A (rather than the A and B I had before).
We are down to matching the Al2O3 and SiO2. Well, not quite matching - I decided to increase both by a little, since I was sure the frit would make the glaze melt better - and thus be able to tolerate, and benefit from them.
To do that I first increase the EPK by three-at-a-time to take the Al2O3 to 0.48 (that's the red number).
Last is the SiO2, the blue number - I increase that enough to get a silica-to-alumina ratio of 9 to 1 (if you want to know about that ratio just click the word "Ratios").

10
There we have it, the chemistry of the improved recipe is doing what I want: Similar to the old, but better.
To test this I printed a batch mix ticket to make 1000 grams.
That was enough to fire test tiles, but also to do this melt fluidity test comparing it to an industrial glaze used in the tableware industry (that is the one on the left). Notice how well our new glaze is melting - this is good news as we will see in a moment.

This looked so nice in initial tests I decided to mix up the original recipe, the one I didn't want to even try, and this one, but with an addition of 10% zircon to opacify them white. Our new fritted version is the one on the left. Notice how much whiter it is - the frit is obviously lower in iron.
Let's look at another picture, this one compares the flow on this G2926A version to the original G2926 - it is flowing better even though I increased the silica and alumina.
Of course, as a normal part of our workflow, I would attach these pictures to the recipe using this button.

11
Then something bad happened: I did a 300 degree to ice water "stress test" on a clay I intended to use it on - unfortunately it crazed like this one.
However, since melting was good there was an opportunity to add silica, plenty of it. Silica is the glass-former in any glaze so the more you can put in the better. And, it reduces thermal expansion. Here is what I did.
First, I duplicated the recipe and code numbered the new one G2926B.
Then I retotaled it to 100, added 10 parts silica as another line and set it to added status.
Then I showed the line order column and brought the talc down to the bottom.
Finally, I clicked "Done Editing".

12
I fired a melt flow test comparing the A and B version. Notice the 10% silica is tolerated really well - only flowing a little less. And, as you can see here on the inside of this mug, it fires super glossy. Better yet, it survived the crazing stress test.
Later on, we made another important improvement, changing to 325 mesh silica. It is not a separate item in the materials database, as you can see I have put the generic name in the "material lookup" fields so the chemistry is still found.
In further testing we accumulated lots of notes. For example, I found that equal parts of powder and water produced a creamy 1.43-1.44 specific gravity slurry that worked well for dipping. And that 1000g produces about 1.4 liters. That would be about 3600g to make a US gallon.
This was intended to emphasize the process that led to the derivation of this popular cone 6 transparent glaze recipe. We did not end up with the exact same recipe (ingredients are at worst 0.5% different, likely because of rounding that was done).



Links

Articles A Low Cost Tester of Glaze Melt Fluidity
Use this novel device to compare the melt fluidity of glazes and materials. Simple physical observations of the results provide a better understanding of the fired properties of your glaze (and problems you did not see before).
Materials Gerstley Borate
Gerstley Borate was a natural source of boron for ceramic glazes. It was plastic and melted clear at 1750F. Now we need to replace it. How?
Recipes G2926B - Cone 6 Whiteware/Porcelain transparent glaze
A base transparent glaze recipe created by Tony Hansen, it fires high gloss and ultra clear with low melt mobility.
Glossary Transparent Glazes
Every glossy ceramic glaze is actually a base transparent with added opacifiers and colorants. So understand how to make a good transparent, then build other glazes on it.
Glossary Glaze Chemistry
Glaze chemistry is the study of how the oxide chemistry of glazes relate to the way they fire. It accounts for color, surface, hardness, texture, melting temperature, thermal expansion, etc.
Typecodes Gerstley Borate Glaze Calculation examples
Examples of how we use glaze calculations (in an Insight-Live.com account) to replace Gerstley Borate with other materials, especially frits, in various glaze recipes. In doing so we take the opportunity to improve the recipe in other ways (e.g. reduce thermal expansion, improve slurry properties, reduce bubbling and crawling).
Typecodes Glaze Chemistry
Case studies where glaze chemistry was used to solve a problem.
Troubles Glaze Crazing
Ask the right questions to analyse the real cause of glaze crazing. Do not just treat the symptoms, the real cause is thermal expansion mismatch with the body.

Cone 6 transparent becomes G2926B:

By surgically removing the Gerstley Borate!


Replacing Gerstley Borate with a frit in a glaze

This picture has its own page with more detail, click here to see it.

These are the original cone 6 Perkins Studio Clear (left) beside our fritted version (right). You cannot just substitute a frit for Gerstley Borate (GB), they have very different chemistries. But, using the calculation tools in my account at insight-live.com, I compensated for the differences by juggling other materials in the recipe. I even upped the Al2O3 and SiO2 a little on the belief that they would dissolve in the more active melt the frit would create. I was right - a melt-flow GLFL test comparison (inset left) shows that the GB version flows less. Using this on ware exhibited another issue (after doing a IWCT test): Crazing. The very good melt flow on my G2926A fritted version is thus good news: It can accept more silica - the more silica, the more durable and craze resistant it will be. How much did it take? 10% more! That ultimately became the recipe for our standard G2926B cone 6 transparent.

Click here for case-studies of Insight-Live fixing problems


Insight-live help button

This picture has its own page with more detail, click here to see it.

You will see examples of replacing unavailable materials (especially frits), fixing various issues (e.g. running, crazing, settling), making them melt more, adjusting matteness, etc. Insight-Live has an extensive help system (the round blue icon on the left) that also deals with fixing real-world problems and understanding glazes and clay bodies.

Gerstley Borate passed on:

It will be missed by many, not by others.


This picture has its own page with more detail, click here to see it.

Near the end, Gerstley Borate first became Costly Borate. The supplier, LagunaClay.com, raised the price to wake us all up to take action in substituting it before supplies ran out. It was a plastic ceramic glaze flux, sourcing boron to melt better than any other common raw material. It had been a foundation material in low and middle temperature pottery glaze recipes for many decades. Potters had a love/hate relationship with it: Enjoying its low melting point but enduring its problems (inconsistency, gelling of the slurry, crawling, micro-bubbles, boron-blue discoloration). Strangely most people used it without knowing what it really was. And few realized how easy it is to replace. Gillespie Borate ended up being the substitute of choice. But it has issues too. The best is to adjust each glaze recipe to source boron from a frit (fixing other issues also).

Please read that last statement carefully. It did not say that there is any frit that can substitute. It said that frits can source boron.

Don't look at the outside of this mug.

The inside is where the magic and potential are!


This picture has its own page with more detail, click here to see it.

This inside glaze is G2926B (on Plainsman M340). It is capable of firing glassy smooth, crystal clear and un-crazed even on coarse stonewares. Watch the video 📹 to see the four unusual things needed to get reliable glazes like this. But the recipe is only part of getting success. Mixing it as a thixotropic slurry is another. And the firing schedule: Look closely at the two glazed tiles. The bottom one, although fired lower (cone 5.5) was slow cooled using the C5DHSC schedule - note how much smoother the glass is (the upper one was fired to cone 6 using the PLC6DS schedule).

The outside is a floating blue, GA6-C. These are a dime a dozen but a good transparent is priceless. Did you know that the outside glaze can be made from the inside one by simply adding 2:4:1 iron oxide:rutile:cobalt oxide? This glaze can be stained, opacified and variegated in an infinite number of ways. And it is adjustable (e.g. lower thermal expansion, lower or higher melting).



Another reason for DIY casting bodies and glazes:

Glaze fit


Four cast porcelain mugs with four different commercial glazes. All crazed!

This picture has its own page with more detail, click here to see it.

These are four different cone 6 commercial glazes made by popular US manufacturers. The body is a cone 6 casting porcelain made by another. All are crazing! This is common. Producer A's glazes fit Producer A's bodies. But not Producer B's. The transparency makes this common issue visible here. But many potters are selling crazed ware. Or ware that will craze over time. Assuming you are not one of them - which company is at fault? Neither. Neither can assure that its product fits those of others.

Mid-fire porcelains commonly craze glazes if they lack sufficient silica (20% is a typical minimum) or don't vitrify. Unfortunately, recipes are proprietary. Wait a minute - these recipes are well-known. You already have a propeller mixer and scale; why not make a DIY porcelain (e.g. L3778D or derivative)? And, why not mix your own transparent brushing glaze or dipping glaze (e.g. G2926B recipe; it has lots of documentation and can be adjusted to deal with fit issues on any clay body)?

G2926B cone 6 transparent liner glaze: Proven, reliable, durable


A hand made pottery mug with clear liner glaze

This picture has its own page with more detail, click here to see it.

While colorful and layered glazes on the outsides of pieces get lots of praise and glory, transparent or white glazes providing the functional surface on the insides of pieces often get little attention from potters. Really, what good is an attractive piece if the food surface is crazing, blistering, leaching or cutlery marking? Or if it converts the piece into a time bomb? This cone 6 liner glaze, G2926B, is an example of how I found a glaze, recognized its potential and then adjusted the recipe to resist crazing on our clay bodies, fire durable and leach resistant and act as a base to host colorants, opacifiers and variegators. I get the best fired results using the C6DHSC firing schedule and very good performance as a dipping glaze when the slurry is thixotropic. One of the reasons this recipe is so widely used is that it is well-documented, having a code number that Google indexes. Drinking from a mug having a quality and fitted functional surface and a nice crisp line dividing the outside and inside glazes instills pride in me as the maker. Watch the G2926B video to see how I developed this. What is the outside glaze? It is the G2934Y matte base recipe plus 8% Mason 6027 stain. The clay is MNP which I make myself.


PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy