Oct 22, 2026: We are working on protecting our servers against the PHP2Shell vulnerability just discovered. The CDN download server is back online. The digitalfire and insight-live servers were patched on Oct 21.

A ChatBot gives jaw-dropping glaze recipe advice - Jan 2025
A Low Cost Tester of Glaze Melt Fluidity
A One-speed Lab or Studio Slurry Mixer
A Textbook Cone 6 Matte Glaze With Problems
Adjusting Glaze Expansion by Calculation to Solve Shivering
Alberta Slip, 20 Years of Substitution for Albany Slip
An Overview of Ceramic Stains
Are You in Control of Your Production Process?
Are Your Glazes Food Safe or are They Leachable?
Attack on Glass: Corrosion Attack Mechanisms
Ball Milling Glazes, Bodies, Engobes
Binders for Ceramic Bodies
Bringing Out the Big Guns in Craze Control: MgO (G1215U)
Can We Help You Fix a Specific Problem?
Ceramic Glazes Today
Ceramic Material Nomenclature
Ceramic Tile Clay Body Formulation
Changing Our View of Glazes
Chemistry vs. Matrix Blending to Create Glazes from Native Materials
Concentrate on One Good Glaze
Converting between Oxide Weight %, Mole % and Unity Formula
Copper Red Glazes
Crazing and Bacteria: Is There a Hazard?
Crazing in Stoneware Glazes: Treating the Causes, Not the Symptoms
Creating a Non-Glaze Ceramic Slip or Engobe
Creating Your Own Budget Glaze
Crystal Glazes: Understanding the Process and Materials
Deflocculants: A Detailed Overview
Demonstrating Glaze Fit Issues to Students
Diagnosing a Casting Problem at a Sanitaryware Plant
Drying Ceramics Without Cracks
Duplicating Albany Slip
Duplicating AP Green Fireclay
Electric Hobby Kilns: What You Need to Know
Fighting the Glaze Dragon
Firing Clay Test Bars
Firing: What Happens to Ceramic Ware in a Firing Kiln
First You See It Then You Don't: Raku Glaze Stability
Fixing a glaze that does not stay in suspension
Formulating a body using clays native to your area
Formulating a Clear Glaze Compatible with Chrome-Tin Stains
Formulating a Porcelain
Formulating Ash and Native-Material Glazes
G1214M Cone 5-7 20x5 glossy transparent glaze
G1214W Cone 6 transparent glaze
G1214Z Cone 6 matte glaze
G1916M Cone 06-04 transparent glaze
Getting the Glaze Color You Want: Working With Stains
Glaze and Body Pigments and Stains in the Ceramic Tile Industry
Glaze chemistry using a frit of approximate analysis
Glaze Recipes: Formulate and Make Your Own Instead
Glaze Types, Formulation and Application in the Tile Industry
Having Your Glaze Tested for Toxic Metal Release
High Gloss Glazes
Hire Us for a 3D Printing Project
How a Material Chemical Analysis is Done
How desktop INSIGHT Deals With Unity, LOI and Formula Weight
How to Find and Test Your Own Native Clays
I have always done it this way!
Inkjet Decoration of Ceramic Tiles
Is Your Fired Ware Safe?
Leaching Cone 6 Glaze Case Study
Limit Formulas and Target Formulas
Low Budget Testing of Ceramic Glazes
Make Your Own Ball Mill Stand
Making Glaze Testing Cones
Monoporosa or Single Fired Wall Tiles
Organic Matter in Clays: Detailed Overview
Outdoor Weather Resistant Ceramics
Painting Glazes Rather Than Dipping or Spraying
Particle Size Distribution of Ceramic Powders
Porcelain Tile, Vitrified Tile
Rationalizing Conflicting Opinions About Plasticity
Ravenscrag Slip is Born
Recylcing Scrap Clay
Reducing the Firing Temperature of a Glaze From Cone 10 to 6
Setting up a Clay Testing Program in Your Company or Studio
Simple Physical Testing of Clays
Single Fire Glazing
Soluble Salts in Minerals: Detailed Overview
Some Keys to Dealing With Firing Cracks
Stoneware Casting Body Recipes
Studio Management Software 2026 (booking)
Substituting Cornwall Stone
Super-Refined Terra Sigillata
The Chemistry, Physics and Manufacturing of Glaze Frits
The Effect of Glaze Fit on Fired Ware Strength
The Four Levels on Which to View Ceramic Glazes
The Majolica Earthenware Process
The Potter's Prayer
The Right Chemistry for a Cone 6 Magnesia Matte
The Trials of Being the Only Technical Person in the Club
The Whining Stops Here: A Realistic Look at Clay Bodies
Those Unlabelled Bags and Buckets
Tiles and Mosaics for Potters
Toxicity of Firebricks Used in Ovens
Trafficking in Glaze Recipes
Understanding Ceramic Materials
Understanding Ceramic Oxides
Understanding Glaze Slurry Properties
Understanding the Deflocculation Process in Slip Casting
Understanding the Terra Cotta Slip Casting Recipes In North America
Understanding Thermal Expansion in Ceramic Glazes
Unwanted Crystallization in a Cone 6 Glaze
Using Dextrin, Glycerine and CMC Gum together
Volcanic Ash
What Determines a Glaze's Firing Temperature?
What is a Mole, Checking Out the Mole
What is the Glaze Dragon?
Where do I start in understanding glazes?
Why Textbook Glazes Are So Difficult
Working with children

Formulating a Porcelain

Description

The principles behind formulating a porcelain are quite simple. You just need to know the purpose of each material, a starting recipe and a testing regimen.

Article

A translucent Polar Ice porcelain mug

Incredible advances have occurred in porcelain manufacturing during recent decades. Robotics, kiln controls, inkjet decoration, pressure casting, isostatic pressing, CNC equipment and 3D printing have transformed production. Yet the material being shaped and fired is still governed by the same fundamentals. A remarkably small number of raw materials can be combined to produce bodies having very different forming behaviour, firing shrinkage, strength, translucency, thermal expansion and resistance to deformation.

Porcelain does not need to be mysterious. A traditional general-purpose porcelain is essentially a highly vitrified, very low-porosity ceramic body made from clean, low-iron and low-titania raw materials. Most are descendants of the classic triaxial porcelain system: clay + feldspathic flux + quartz. During firing, feldspar-derived liquid promotes densification and dissolves portions of the other particles; on cooling, the fired body consists mainly of a glassy matrix containing mullite crystals and residual quartz.

Unlike a glaze, a porcelain cannot be understood very well from its oxide formula alone. Mineralogy, particle size and shape, plasticity, packing, grinding, forming method and firing history are often just as important as chemistry. For this reason, porcelain formulation is largely about measuring physical properties and adjusting the recipe to control them.

A general-purpose plastic porcelain normally contains:

Special-purpose porcelains can depart considerably from this traditional system. Alumina can replace some or much of the quartz where greater hardness, strength or resistance to quartz-related thermal effects is required. Alumina porcelains can be substantially stronger than conventional quartz porcelains, although their thermal expansion behaviour depends on the complete formulation and fired microstructure rather than simply the alumina percentage.

Frits and other powerful fluxes can supplement or replace feldspar where a lower vitrification temperature is required. Organic binders, plasticizers and lubricants become much more important in low-clay dry-pressing bodies because forming strength need not come entirely from plastic clay. Minerals such as pyrophyllite can also be employed where dimensional stability and thermal-expansion characteristics justify departing from the conventional quartz-kaolin-feldspar system.

The whitest and most translucent porcelains are almost always made using the most expensive materials (because the expense is a product of achieving low iron levels). These can keep the body white even where lots of glass development occurs.

The "Universal 25 Porcelain" recipe typically produces an inexpensive cone 10 not-very-white porcelain having moderate plasticity and near zero porosity. It is made from 25% each of ball clay, kaolin, feldspar, and silica, or more simply, 50% clay and 25% each of silica and feldspar. Thousands of potters and manufacturers use this "as is" using the brand name materials they have access to. Let's consider some physical properties to look for in a porcelain (not ordered in any specific way).

Translucent vs non-translucent porcelain

Porcelains can be compared in all of the above areas. Testing is needed to find property balances. Most physical properties can be measured or at least compared using simple equipment, methods and observations. Let's look again at each of the materials in the recipe.

Pure #6 Tile kaolin can be thrown like a pottery clay

Kaolin

A true porcelain would normally derive all its plasticity from a kaolin. Since kaolins are often of limited plasticity, this limits the workability of throwing or modeling porcelains made from them. Still, there are some surprisingly plastic kaolins, although the limited range of particle sizes can mean less than ideal drying performance. Do not accept that a kaolin is plastic just because its name includes the word plastic or a supplier says it is plastic, test yourself. For casting porcelains, an all-kaolin approach is quite feasible (using 50% kaolin rather than 25% kaolin and 25% ball clay) since these bodies benefit greatly from the reduced drying shrinkage and increased water permeability associated with the larger particle size of kaolins. However an all-kaolin casting porcelain may not have the strength to pull away from the plaster mold without cracking, add a little plasticizer if needed.

Kaolins can differ widely in maturity. British kaolins require the use of less feldspar because they already have some natural fluxes as part their mineral particle profile. So even though these might be less plastic, less flux is needed, so more kaolin can be used in a recipe. It is an good idea to make up the kaolin complement of a recipe using more than one brand, this provides a better distribution of ultimate particle sizes and minimizes the effect on the body if one kaolin changes.

Since kaolins vary quite widely in their plasticity, maturity, soluble salts, particle size and whiteness, it can be quite a challenge to test and classify them all. Data sheets are often not that helpful because they present information in different ways and seldom does a company explain its materials in terms of other well known alternatives. The burden of picking the best kaolins thus rests on you and your ability to evaluate and compare them using tests that document the appropriate physical properties. We recommend you use the DFAC test, SHAB test, and LDW test to compare kaolins (and ball clays).

About casting bodies: Larger particle size kaolins tend to be dirtier, less plastic, more expensive and have lower dry strength, so their benefits come at a cost. It is possible to make fairly fast-casting zero-ball-clay bodies with ordinary light burning kaolins like EPK. Some companies use large-particle-size kaolin when they also have ball clay in the mix, the latter may be canceling the benefit of the former! Of course large particle ball clays are also available, but remember that they are still considerably finer than standard kaolins. Also, fine-tuning a kaolin mix makes little sense if the body is not deflocculated properly. The best approach is to use a standard white burning kaolin, deflocculate it properly and learn to work with it. Then fine tune it by the substitution of some large particle material to speed casting rate while watching for any deleterious properties introduced.

Following is a sample of a Foresight report on a kaolin (Foresight was the predecessor to insight-live.com). I have tested using DFAC, SHAB, LDW and SIEV tests.

Ball Clay & Bentonite

OM4 Ball Clay fired cone 10R and 10 down to 4 oxidation

Ball clay is much finer and thus much more plastic than kaolin. A very wide range of ball clays are available. White burning ball clays should not have near the plasticity of their dirtier counterparts - but often they do! Bentonite is much finer than ball clay (the ultimate particles are much smaller). It is incredibly plastic, adding only 2% to a recipe can drastically improve working properties. However, these materials have a down side. Ball clays can have ten times the amount of brown-firing iron oxide that kaolin has and many have soluble salts that can produce a scum on the burned surface. Many also contain lignite particles that can produce glaze imperfections. Raw bentonites can be downright dirty, burning brown or red with possible specking and soluble salts sometimes so heavy they form a glaze. White firing bentonites come in a wide range of plasticities. Some have so little plasticity one wonders why anyone would use them for ceramics, others are incredibly plastic. But beware, even though only 3-5% might be used, the cost of this one material could be more than the other 95% combined! A study of all the ball clays and bentonites available in your area can be a real education! Again it is important that you have a testing regimen to compare and characterize these materials (e.g. a group account at Insight-Live.com). There is another up-side of ball clay worth mentioning. Ball clays contain free silica, so if there is significant ball clay in a recipe the silica can be reduced leaving room to add more clay for plasticity or feldspar for maturity.

So the easiest way to increase the plasticity of the standard '25 Porcelain' is to add 2%-3% raw bentonite. Even though most inexpensive 200 mesh bentonites can be quite dirty, this small amount may not affect the fired color as much as expected. Do not overlook one detail: Bentonite is difficult to process, one bag of raw bentonite may not contain iron specks while the next does not. Microfine ceramic grades (e.g. 600 mesh) are available, but obviously are much more expensive. If whiteness is not all-important, increase the ball clay at the expense of kaolin to produce a plastic whiteware (feldspar percentage may need reduction also, ball clay is less refractory than kaolin). For a very white porcelain, the challenge will likelybe reducing or entirely eliminating the ball clay. Where super whiteness is secondary to having a good general purpose body, some ball clay can usually be tolerated. If having the most plastic body possible is the most important, then use all ball clay and no kaolin (e.g. B-Mix from Laguna), that brings awesome workability also.

Feldspars (and Nepheline Syenite)

Feldspar vs Nepheline Syenite melt fluidity test

These are the fluxes, or more correctly, contain the fluxes. Fluxes are the oxides that help develop fired maturity by liquefying and slowly dissolving some of the clay and silica. The total flux amount necessary is easily determined by simply firing to a range of temperatures above and below the intended; studying the absorption, strength, and firing shrinkage curves; and adjusting the amount of feldspar to give the desired maturity. The amount of feldspar for a cone 10 body varies from 15%-30%, depending on the other materials in the recipe. For a typical American kaolin, it takes about 25% for cone 10 and up to 50% for cone 6.
Feldspars are not without potential problems. While some brands can be relatively iron free, others fire surprisingly darker. Some can present flocculation problems due to slight solubility. Sodium feldspars are generally cleaner and more potent. Use two or three together if possible (to dampen changes that could occur in one).

Silica

When silica is inadequate this happens

Silica tends to be a very consistent and inexpensive material. Quartz grains act primarily as a micro-aggregate or framework structure for the fired matrix. In addition, some of the silica particle and particle edges are dissolved by the fluxes to produce aluminum-silicate glasses. Too much silica in a recipe could mean lower plasticity (since less room is left for clay). However, there is also much discussion about the detrimental effects of crystobalite (i.e. dunting), whose development during high temperature firing is related to available free quartz. Thus there is some merit to lower silica amounts, especially if you have the ability to adjust your glazes to lower their expansion. The use of less silica means more clay can be added resulting in higher plasticity. A finer silica (300 mesh) reacts better with the fluxes and thus less is needed (but thermal expansion drops). Too little silica in a body can mean crazing glazes since the quartz mineral contributes to higher expansion that assists glaze fit. Of course, lack of silica will also mean more of a tendency to warp during firing. For cone 10, many technicians aim at 20-25% for expansion reasons and to provide firing stability over a range of temperatures.

Recipes & Strategies

Most people have noted that the '25 Plastic Porcelain' recipe has flaws that can be corrected for individual situations and materials. To improve this recipe for cone 10:

To formulate a white translucent cone 6 plastic porcelain:

For a casting porcelain, remember that much lower plasticity is needed. Common consensus in industry is that it is much more important to use kaolins of large particle size, so water can easily be drawn out by the plaster mold. However for a smaller operation that does not need to really optimize mold release time, normal kaolins are fine. The cleanest kaolins and ball clays are also the least plastic, thus casting porcelains (that can tolerate this) can achieve whiter and more translucent effects than their plastic counterparts. It is imperative to understand the principles of deflocculation so that the amount of water in the slurry can be minimized and proper mold release and casting time can be achieved. To cast very thin ware some bentonite May be needed (start with 1%) to give it the strength to pull itself away from the mold during drying.

For plastic porcelain for modelling or throwing pay careful attention to drying properties. Since porcelains are fine-grained, they don't usually dry well, thus plastic porcelains are even worse. Add just enough bentonite to give the plasticity needed (the DFAC test can be handy for this). Some people add molochite grog to porcelains for better drying.

Give careful thought to how mature the porcelain needs to fire. If zero absorption is not necessary, consider reducing the feldspar to get more plasticity from the clays (and be able to reduce the bentonite). Such a body can still be considered functional and vitreous and it will resist warping in the kiln. In addition, material changes that result in more maturity will be less likely to cause trouble in a body that has some 'room to move'. Measure fired absorption at a variety of temperatures (a 'measure-only-at-the-working-temperature' philosophy is a tunnel vision approach that will almost certainly get you into trouble, especially in situations where the working temperature is far above the point at which zero porosity is attained).

Trade-offs to consider when formulating or adjusting a plastic porcelain.

Material Typical % Details
Silica 20%-25% Use at least 20% (more for high expansion glazes, less for low). For maximum translucency use less (less silica permits more feldspar)
Flux Feldspar body
Cone 10: 25% feldspar
Cone 6: 35% feldspar


Frit body
Cone 10:10%
Cone 6: 20%
Use the amount required for the degree vitrification and translucency needed.
Kaolin Cone 10: 25%-50%
Cone 6: 20%-40%.
Ideally, use as much kaolin and as little ball clay as possible (for firing whiteness). Test various types for the best combination of whiteness and plasticity.
Ball Clay Up to 25% Ball clays impart plasticity but are higher in iron and detrimentally effect fired whiteness. Doing detailed fired and workability comparisons of brand names can really pay off. If necessary, add barium carbonate (for the ball clay proportion) to precipitate solubles.
Plasticizers Plastic bodies: 2-4%
Casting bodies:0-1%
Bentonites are cheapest. Highly processed smectites and hectorites are most expensive. The best quality products are twenty or thirty times more expensive than the cheapest. Do tests to find a compromise between impact on fired color, plasticity gained and cost.

Bone China

These are fired around 1250C bisque and glazed between 1050 and 1100C. One composition we know of is 45% bone, 30% clay and 25% mix of potash feldspar and quartz. But lower bone versions are used also, it being as low as 10% (the clay is the same but the feldspar obviously has to be much higher). It is not completely clear why companies do not simply add frit to a standard white porcelain to get translucency. If you know this, please email me.

Money-Is-No-Object Recipe

Frit can be used to mature a porcelain, Zero4 porcelain is an example.

Related Information

Mix a cone 6 porcelain test:

Step 1: Conquer the mental block


Red burning porcelain test being prepared

This picture has its own page with more detail, click here to see it.

This is L4588 red burning porcelain. I got the idea after coffee break and was rolling and pressing specimens right after lunch. How?

The major reason is not being intimidated by mixing body and glaze tests. Another is having all the tools and materials close at hand (shown here). Third is a good record-keeping system where I make sure to enter results, notes, pictures and links to related tests at every stage of a project.

A plaster table: Better than a pugmill, essential for testing


A plaster table

This picture has its own page with more detail, click here to see it.

This is an example of an angle iron utility table being made into a plaster table. The cardboard sides extend upward to make the slab thicker and create a buffer gap to prevent the expanding and setting plaster from pressing outward on the frame. 150 lbs plaster (92 lbs water) was poured into the plastic-lined space (the bottom cardboard sections were supported from below). In a dry enough climate, this table could make enough clay to support slurry-to-plastic production for a potter (a thicker slab and a fan would enable even more capacity). The slurry-up process is better than a pugmill for small operations. It's much cheaper and is an easier way to utilize scrap material and weigh out custom recipes. The clay quality and de-airing is better (without hard chunks and contamination common to pugmilling). The procedure generates much less dust and the tank is easily cleaned. Slurries are easily sieved, especially if you have a sieve shaker.

DIY clay bodies via slurry mixing:

Consider the advantages.


This picture has its own page with more detail, click here to see it.

Consider the advantages of making your own clay bodies using a propeller mixer and plaster table.
-Independence: You control product availability, quality and consistency.
-Flexibility: You control the recipe (with our help if needed). Fine-tune and adjust it over time to fit your needs and compensate for variations in material properties and supply.
-Special-purpose clay bodies are possible, ones that ceramic suppliers do not or cannot make.
-The slurry up process achieves better mixing and deairing than any pugmill. No aging needed.
-A mixer and plaster table are useful for so many other things in a pottery studio.
-Achieving the right stiffness is an integral part of the process.
-Recycling scrap, by slaking, fits the process.
-Local native clays: Slurries enable the use of a magnet to remove iron, a sieve to remove particulates and a settling process to remove soluble salts.
-Cleanup is easy so many kinds of clay can be made without cross contamination.
-It is rewarding - you will own the whole process, the bragging rights alone make it worthwhile for me!

Silica in porcelain recipes kills two birds with one stone:

To demonstrate, here's what happens when you leave it out


A porcelain cup with serious crazing and base crack concentric to the center

This picture has its own page with more detail, click here to see it.

This body is 70:30 kaolin:feldspar (fired at cone 6 with glaze G2926B). The fired body has a vitreous porcelain-like surface. But, this dense craze pattern indicates a very serious fit problem. The COE (thermal expansion) of this body is much too low, primarily because there is no residual quartz. There isn't a glaze-fix solution to this. Reformulating it enough to fit, while maintaining the firing characteristics, would be well beyond the expertise, material availability and budget of any typical pottery or manufacturer. All that work would just boil down to "compensating for an unusually low-expansion body". Adding quartz to the body to raise its COE is the appropriate conventional solution. An initial test would be to substitute 25 of the kaolin for 200 mesh silica. It is refractory, and while the finer particles will be dissolved by the feldspar, enough of the larger pure quartz ones will remain to impose their very high COE on the fired matrix.

The other issue is with the flat particle shape of kaolin. The throwing process has lined up the predominant kaolin particles concentric to the centre. During drying, and especially firing, more shrinkage occurs across them than along them. All ten of the cups, which I made and dried in my normal, careful fashion, cracked like this! The solution is adding a filler, one with non-platy particles. Silica is perfect; the grains act like aggregate in concrete, strengthening the matrix and separating the clay particles, forcing them to orient more randomly.

NZ kaolin-based slip casts at 1mm thickness. How?


A very thin walled porcelain bowl

This picture has its own page with more detail, click here to see it.

This is Polar Ice casting, a cone 6 translucent porcelain that uses New Zealand Halloysite. The base body recipe would never have enough plastic strength to pull itself from this mold without tearing. But the addition of 1% Veegum gives it amazing strength. This dried cast bowl measures 130mm in diameter and 85mm deep; it only weighs 89 gm! The slip was in the mold for only 1 minute before pour-out. Of course, there is a price to pay for adding the Veegum: Increased casting time and more difficult deflocculation. This 1% addition can be refined. A program of testing could indicate that a lower percentage of Veegum could work, increasing the casting rate. The polar ice information page has very good information, under the heading “Casting Recipe” (it deals with the trade-offs of using this kaolin in casting bodies).

Now that is a translucent porcelain! But much more.


Polar Ice porcelain mug with a light inside to demonstrate its translucency

This picture has its own page with more detail, click here to see it.

These are two cone 6 transparent-glazed porcelain mugs. On the left is the porcelainous Plainsman M370 (Laguna B-Mix 6 would have similar opacity - none). Right is the highly vitreous, New Zealand kaolin-based porcelain, Polar Ice. The secret to making this porcelain super-white is the NZ kaolin. The secret of its impossibly high plasticity is the very expensive plasticizer, VeeGum T. What about the translucency? That is a little more complicated. Nepheline syenite is used as the feldspar, but it alone, in a practical recipe, cannot deliver this kind of translucency at cone 6. Amazingly, the 4% Veegum acts as a translucency catalyst; it is the real secret. Commercial manufacturers could never use a sticky and difficult-to-dry porcelain like this, but a potter can do incredible things with it (e.g. throw thinner, lighter, bigger than any other clay he/she has ever used!). Can you make this? Yes. Try the L3778D or L3778G recipes.

Clay is dirt. Glaze is powdered rock and glass.

Why do they cost so much? DIY is the answer.


Shipping containers piled high

This picture has its own page with more detail, click here to see it.

Historically, pottery has been a shining star of resilience and independence because the materials were in the ground nearby. So why are they coming thousands of miles in shipping containers? Because you can't just head out to the nearest hill with your wheelbarrow. But you are not helpless either.

Rather than viewing these containers as full of specific brand-name clays, minerals and man-made powders, it is better to view them as full of materials that supply the physical properties and chemistries needed to make bodies, glazes, engobes, slips, etc. By characterizing your glazes and bodies, using an effective record-keeping system, you can not only adjust recipes to adapt to changing supplies, but even improve them in the process (adjusting glaze thermal expansion, temperature, surface, color, etc). Or, use materials native to your area. It is not rocket science; it is just work and gradual learning accompanied by organized record-keeping, good labelling and interpretation skills.

Potter goes full DIY and makes her own porcelain

The best thing happens: Failure on the third mix!


Blistered porcelain mug

This picture has its own page with more detail, click here to see it.

Super white translucent porcelains are expensive, approaching $200/box in some countries! Even so, variation in properties is common (certainly not good for a "tipping point body" that is difficult to make). The idea of making your own clay body is actually feasible here. Yet Kirsty Kash, maker of this mug, told me that this amount of DIY was something she had never really considered, thinking it would be too complicated without guidance. But ongoing issues with the commercial clay gave her the motivation to give it a try (using a recipe similar to L3778D). She weighed out the materials, slurried up the mix using a propeller mixer, finished by blender mixing and then dewatered on a super-clean plaster bat.

By the third batch, something good happened: The porcelain blistered (tiny bumps on the surface). Subsequent correspondence brought the realization that this type of body is "walking a recipe tightrope" that requires control of the percentage of the key ingredient: Feldspar. It determines the maturity of the fired product. Too much brings blisters, too little and translucency is lost. Simple testing is all that is needed to determine the needed amount. More good news: The change enabled increasing the kaolin percentage by the same amount. That, in turn, enabled reducing the percentage of veegum (reducing the cost).

Her comment a few days ago was inspiring: "I'm getting to know my material so intimately. I have been learning SO much." When I suggested she might end up buying commercial again she responded: "I just bought large bags of all the materials and plan to keep going. I like having the control and being less reliant on the boxed clay. You've converted me!".

Links

Articles Stoneware Casting Body Recipes
Some starting recipes for stoneware and porcelain with information on how to adjust and adapt them
Articles Rationalizing Conflicting Opinions About Plasticity
How can two potters have completely different opinions about the plasticity and workability characteristics of the same clay body
Materials Feldspar
In ceramics, feldspars are used in glazes and clay bodies. They vitrify stonewares and porcelains. They supply KNaO flux to glazes to help them melt.
Materials Veegum
A clay of incredibly small particle size. It has the highest plasticity of any known clay and acts as a suspending and gelling agent in slurries.
Materials Kaolin
The purest of all clays in nature. Kaolins are used in porcelains and stonewares to impart whiteness, in glazes to supply Al2O3 and to suspend slurries.
Materials Silica
Silica, sold as a white powder, is pure quartz mineral. Quartz is pure SiO2 silicon dioxide. It is the most abundant mineral on earth and most used in ceramics.
Materials Ball Clay
A fine particled highly plastic secondary clay used mainly to impart plasticity to clay and porcelain bodies and to suspend glaze, slips and engobe slurries.
Materials Bentonite
Bentonite can make a clay body instantly plastic, only 2-3% can have a big effect. It also suspends slurries so they don't settle out and slows down drying.
Materials Hectorite
A sodium magnesium montmorillonite that burns much whiter than bentonite (because of lower iron content).
Materials HPM-20 Volclay Bentonite
Materials Ferro Frit 3110
High sodium, high thermal expansion low boron frit. A super-feldspar in clay bodies. Melts at very low temperatures. Useful to make crackle glazes.
Properties Body Maturity
Tests Shrinkage/Absorption Test
SHAB Shrinkage and absorption test procedure for plastic clay bodies and materials
Tests Soluble Salts
Evaluate and compare the solubles salts content in clay bodies and materials
Tests Drying Factor
The DFAC Drying Factor test visually displays a plastic clay's response to very uneven drying. It is beneficial to show the relative drying performance of different clays.
Tests LOI/Density/Water Content
LDW LOI, density and water content test procedure for plastic clay bodies and porcelains
Tests Drying Factor/Water Content/Solubles
Tests 300F:Ice Water Crazing Test
Ceramic glazes that do not fit the body often do not craze until later. This progressively stresses the fit until failure point, thus giving it a score
Glossary Porcelain
How do you make porcelain? There is a surprisingly simple logic to formulating them and to adjusting their working, drying, glazing and firing properties for different purposes.
Glossary Sintering
A densification process occurring within a ceramic kiln. With increasing temperatures particles pack tighter and tighter together, bonding more and more into a stronger and stronger matrix.
URLs https://digitalfire.com/university/insight-live/overview/Insight-Live%20Overview.html
Insight-Live.com Overview Video
Recipes L2000 - 25 Porcelain
Base 25x4 porcelain recipe

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy