A ChatBot gives jaw-dropping glaze recipe advice - Jan 2025A Low Cost Tester of Glaze Melt FluidityA One-speed Lab or Studio Slurry MixerA Textbook Cone 6 Matte Glaze With ProblemsAdjusting Glaze Expansion by Calculation to Solve ShiveringAlberta Slip, 20 Years of Substitution for Albany SlipAn Overview of Ceramic StainsAre You in Control of Your Production Process?Are Your Glazes Food Safe or are They Leachable?Attack on Glass: Corrosion Attack MechanismsBall Milling Glazes, Bodies, EngobesBinders for Ceramic BodiesBringing Out the Big Guns in Craze Control: MgO (G1215U)Can We Help You Fix a Specific Problem?Ceramic Glazes TodayCeramic Material NomenclatureCeramic Tile Clay Body FormulationChanging Our View of GlazesChemistry vs. Matrix Blending to Create Glazes from Native MaterialsConcentrate on One Good GlazeConverting between Oxide Weight %, Mole % and Unity FormulaCopper Red GlazesCrazing and Bacteria: Is There a Hazard?Crazing in Stoneware Glazes: Treating the Causes, Not the SymptomsCreating a Non-Glaze Ceramic Slip or EngobeCreating Your Own Budget GlazeCrystal Glazes: Understanding the Process and MaterialsDeflocculants: A Detailed OverviewDemonstrating Glaze Fit Issues to StudentsDiagnosing a Casting Problem at a Sanitaryware PlantDrying Ceramics Without CracksDuplicating Albany SlipDuplicating AP Green FireclayElectric Hobby Kilns: What You Need to KnowFighting the Glaze DragonFiring Clay Test BarsFiring: What Happens to Ceramic Ware in a Firing KilnFirst You See It Then You Don't: Raku Glaze StabilityFixing a glaze that does not stay in suspensionFormulating a body using clays native to your areaFormulating a Clear Glaze Compatible with Chrome-Tin StainsFormulating a PorcelainFormulating Ash and Native-Material GlazesG1214M Cone 5-7 20x5 glossy transparent glazeG1214W Cone 6 transparent glazeG1214Z Cone 6 matte glazeG1916M Cone 06-04 transparent glazeGetting the Glaze Color You Want: Working With StainsGlaze and Body Pigments and Stains in the Ceramic Tile IndustryGlaze chemistry using a frit of approximate analysisGlaze Recipes: Formulate and Make Your Own InsteadGlaze Types, Formulation and Application in the Tile IndustryHaving Your Glaze Tested for Toxic Metal ReleaseHigh Gloss GlazesHire Us for a 3D Printing ProjectHow a Material Chemical Analysis is DoneHow desktop INSIGHT Deals With Unity, LOI and Formula WeightHow to Find and Test Your Own Native ClaysI have always done it this way!Inkjet Decoration of Ceramic TilesIs Your Fired Ware Safe?Leaching Cone 6 Glaze Case StudyLimit Formulas and Target FormulasLow Budget Testing of Ceramic GlazesMake Your Own Ball Mill StandMaking Glaze Testing ConesMonoporosa or Single Fired Wall TilesOrganic Matter in Clays: Detailed OverviewOutdoor Weather Resistant CeramicsPainting Glazes Rather Than Dipping or SprayingParticle Size Distribution of Ceramic PowdersPorcelain Tile, Vitrified TileRationalizing Conflicting Opinions About PlasticityRavenscrag Slip is BornRecylcing Scrap ClayReducing the Firing Temperature of a Glaze From Cone 10 to 6Setting up a Clay Testing Program in Your Company or StudioSimple Physical Testing of ClaysSingle Fire GlazingSoluble Salts in Minerals: Detailed OverviewSome Keys to Dealing With Firing CracksStoneware Casting Body RecipesStudio Management Software 2026 (booking)Substituting Cornwall StoneSuper-Refined Terra SigillataThe Chemistry, Physics and Manufacturing of Glaze FritsThe Effect of Glaze Fit on Fired Ware StrengthThe Four Levels on Which to View Ceramic GlazesThe Majolica Earthenware ProcessThe Potter's PrayerThe Right Chemistry for a Cone 6 Magnesia MatteThe Trials of Being the Only Technical Person in the ClubThe Whining Stops Here: A Realistic Look at Clay BodiesThose Unlabelled Bags and BucketsTiles and Mosaics for PottersToxicity of Firebricks Used in OvensTrafficking in Glaze RecipesUnderstanding Ceramic MaterialsUnderstanding Ceramic OxidesUnderstanding Glaze Slurry PropertiesUnderstanding the Deflocculation Process in Slip CastingUnderstanding the Terra Cotta Slip Casting Recipes In North AmericaUnderstanding Thermal Expansion in Ceramic GlazesUnwanted Crystallization in a Cone 6 GlazeUsing Dextrin, Glycerine and CMC Gum togetherVolcanic AshWhat Determines a Glaze's Firing Temperature?What is a Mole, Checking Out the MoleWhat is the Glaze Dragon?Where do I start in understanding glazes?Why Textbook Glazes Are So DifficultWorking with children
Making Glaze Testing Cones
Description
A standard shape and size of glaze test is important to be able to compare one test with another, especially over time (so that old tests look the same as new ones)
Article
Joe Schmidt, lab technician at Plainsman Clays, developed the glaze testing cone, it is very practical. It is a standard shape and size that is always used, this serves well for comparison and documentation purposes.
Advantages
- They are easy to make.
- They are easy to photograph
- They are stable and less likely to tip over and break
- They stack well in boxes
- They display a glaze in a way that is akin to a piece of pottery or ceramic.
Steps to make these:
- Print the pattern and cut it out
- Roll the clay to 1/4 inch (6mm) thickness
- Cut the shape out of the clay using the pattern
- Apply a band of slip to one end and attach the other using a 15mm (1/2 inch overlap)
- Press the joint firmly together (use a stick on the inside to support) and press the indentations
- Dry the clay to leather hardness and carve a design on the side opposite the join (to show what it does on edges, in varying thickness around contours and on an uneven surface)
- Stamp the identification of the clay at the bottom
- Dry the testers carefully to avoid cracking
- Use a knife to trim off any sharp edges
- Bisque fire.
When dipping these in glaze consider the following:
- Dip down to within 15mm (1/2 inch) of the base
- Label clearly on the bare clay section
- Dip the top half again for a double-thickness.
Pattern
Use the link below to download the pattern file.
Related Information
An example of the value of a good glaze testing sample.

This picture has its own page with more detail, click here to see it.
These are made at Plainsman Clays in Alberta, Canada.
Preparing to make a glaze testing cone: cutting around the pattern

This picture has its own page with more detail, click here to see it.
In this picture a piece of cardboard is used as a template, you can download a pattern using the URL link on this page.
Making a glaze testing cone: applying the slip for the join.

This picture has its own page with more detail, click here to see it.
A viscous slip will make a better join and minimize the chance of water-splits developing at the edge of the overlap.
Making a glaze testing cone: finishing the join.

This picture has its own page with more detail, click here to see it.
With most clays no scoring is needed, the slip and pressure are enough to make a good join.
Making a glaze testing cone: Incising the surface

This picture has its own page with more detail, click here to see it.
Glaze thickness thins on the edges of the incised lines and thickens at their bases. This enables variegating glazes to showcase their visual effect with varying thickness. And these test the ability of opaque glazes to still cover well when the layer is thin.
Making a glaze testing cone: Stamping an identification.

This picture has its own page with more detail, click here to see it.
The code numbers get recorded with the pictures in our testing system (an account at insight-live.com).
 PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
|
By Tony Hansen Follow me on
 |  |
Got a Question?
Buy me a coffee and we can talk 
https://digitalfire.com, All Rights Reserved
Privacy Policy