A ChatBot gives jaw-dropping glaze recipe advice - Jan 2025
A Low Cost Tester of Glaze Melt Fluidity
A One-speed Lab or Studio Slurry Mixer
A Textbook Cone 6 Matte Glaze With Problems
Adjusting Glaze Expansion by Calculation to Solve Shivering
Alberta Slip, 20 Years of Substitution for Albany Slip
An Overview of Ceramic Stains
Are You in Control of Your Production Process?
Are Your Glazes Food Safe or are They Leachable?
Attack on Glass: Corrosion Attack Mechanisms
Ball Milling Glazes, Bodies, Engobes
Binders for Ceramic Bodies
Bringing Out the Big Guns in Craze Control: MgO (G1215U)
Can We Help You Fix a Specific Problem?
Ceramic Glazes Today
Ceramic Material Nomenclature
Ceramic Tile Clay Body Formulation
Changing Our View of Glazes
Chemistry vs. Matrix Blending to Create Glazes from Native Materials
Concentrate on One Good Glaze
Converting between Oxide Weight %, Mole % and Unity Formula
Copper Red Glazes
Crazing and Bacteria: Is There a Hazard?
Crazing in Stoneware Glazes: Treating the Causes, Not the Symptoms
Creating a Non-Glaze Ceramic Slip or Engobe
Creating Your Own Budget Glaze
Crystal Glazes: Understanding the Process and Materials
Deflocculants: A Detailed Overview
Demonstrating Glaze Fit Issues to Students
Diagnosing a Casting Problem at a Sanitaryware Plant
Drying Ceramics Without Cracks
Duplicating Albany Slip
Duplicating AP Green Fireclay
Electric Hobby Kilns: What You Need to Know
Fighting the Glaze Dragon
Firing Clay Test Bars
Firing: What Happens to Ceramic Ware in a Firing Kiln
First You See It Then You Don't: Raku Glaze Stability
Fixing a glaze that does not stay in suspension
Formulating a body using clays native to your area
Formulating a Clear Glaze Compatible with Chrome-Tin Stains
Formulating a Porcelain
Formulating Ash and Native-Material Glazes
G1214M Cone 5-7 20x5 glossy transparent glaze
G1214W Cone 6 transparent glaze
G1214Z Cone 6 matte glaze
G1916M Cone 06-04 transparent glaze
Getting the Glaze Color You Want: Working With Stains
Glaze and Body Pigments and Stains in the Ceramic Tile Industry
Glaze chemistry using a frit of approximate analysis
Glaze Recipes: Formulate and Make Your Own Instead
Glaze Types, Formulation and Application in the Tile Industry
Having Your Glaze Tested for Toxic Metal Release
High Gloss Glazes
Hire Us for a 3D Printing Project
How a Material Chemical Analysis is Done
How desktop INSIGHT Deals With Unity, LOI and Formula Weight
How to Find and Test Your Own Native Clays
I have always done it this way!
Inkjet Decoration of Ceramic Tiles
Is Your Fired Ware Safe?
Leaching Cone 6 Glaze Case Study
Limit Formulas and Target Formulas
Low Budget Testing of Ceramic Glazes
Make Your Own Ball Mill Stand
Making Glaze Testing Cones
Monoporosa or Single Fired Wall Tiles
Organic Matter in Clays: Detailed Overview
Outdoor Weather Resistant Ceramics
Painting Glazes Rather Than Dipping or Spraying
Particle Size Distribution of Ceramic Powders
Porcelain Tile, Vitrified Tile
Rationalizing Conflicting Opinions About Plasticity
Ravenscrag Slip is Born
Recylcing Scrap Clay
Reducing the Firing Temperature of a Glaze From Cone 10 to 6
Setting up a Clay Testing Program in Your Company or Studio
Simple Physical Testing of Clays
Single Fire Glazing
Soluble Salts in Minerals: Detailed Overview
Some Keys to Dealing With Firing Cracks
Stoneware Casting Body Recipes
Studio Management Software 2026 (booking)
Substituting Cornwall Stone
Super-Refined Terra Sigillata
The Chemistry, Physics and Manufacturing of Glaze Frits
The Effect of Glaze Fit on Fired Ware Strength
The Four Levels on Which to View Ceramic Glazes
The Majolica Earthenware Process
The Potter's Prayer
The Right Chemistry for a Cone 6 Magnesia Matte
The Trials of Being the Only Technical Person in the Club
The Whining Stops Here: A Realistic Look at Clay Bodies
Those Unlabelled Bags and Buckets
Tiles and Mosaics for Potters
Toxicity of Firebricks Used in Ovens
Trafficking in Glaze Recipes
Understanding Ceramic Materials
Understanding Ceramic Oxides
Understanding Glaze Slurry Properties
Understanding the Deflocculation Process in Slip Casting
Understanding the Terra Cotta Slip Casting Recipes In North America
Understanding Thermal Expansion in Ceramic Glazes
Unwanted Crystallization in a Cone 6 Glaze
Using Dextrin, Glycerine and CMC Gum together
Volcanic Ash
What Determines a Glaze's Firing Temperature?
What is a Mole, Checking Out the Mole
What is the Glaze Dragon?
Where do I start in understanding glazes?
Why Textbook Glazes Are So Difficult
Working with children

Are Your Glazes Food Safe or are They Leachable?

Description

Many potters do not think about leaching, but times are changing. What is the chemistry of stability? There are simple ways to check for leaching, and fix crazing.

Article

We live in a 'no fault' world. People tend to blame others for things. For example, it is fashionable to blame alcoholism and criminal behavior on our genes now. However, if your pottery is leaching harmful compounds into food a drink, there is no one to blame but you. To be honest, you probably like to take the credit for your designs. Then you should also take responsibility. If you can calculate the oxide formula of your glaze and do a couple of simple tests you will be in the best good position to defend your use of them.

There is definitely a school-of-thought in both industrial and hobby ceramics that the 'leaching glaze' issue is totally overblown. Thus, if there is pottery leaching harmful compounds into food and drink, it is being produced both by companies and people that do not know any better and who have made a conscious choice to ignore the issue.

The US FDA (Food and Drug Administration) tests ceramic ware extensively for leaching metals often with distressing results. After a meeting and lunch with their representative at the American Ceramic Society convention I was very encouraged by their position on this matter. While they are ready to take action against offenders, they are much more anxious to see initiatives by companies and potters to learn how to recognize leach-likely processes, materials, and formulations and learn how to fix the problems.

There are lots of things we don't know about leaching in glazes. However what follows are some things we do know.

Glazes are glass and we tend to think of them as timeless, indestructible. However all glass leaches to some extent when it comes into contact with even water. With acids, especially if the contact occurs over a period of time or the acid is hot, the effect is obviously greater. Vandals, for example, simply use sulfuric acid in bingo doppers to etch grafitti into windows. This is evident by a change in the gloss and texture of the glass surface over time. Glaze color can change also. As a demonstration try 33% CaO, 42% B2O3, 6% Al2O3 & 18% SiO2 at 950C. It should fizz and dissolve in vinegar within minutes even though it fires to a clear and apparently hard surface.

If a glaze is made from harmless materials like silica, dolomite, kaolin, feldspar, whiting, ball clay, etc. leaching is only a functional and aesthetic issue. But if the glaze employs metallic colorants (other than iron) or other minerals containing lithium, barium, lead, chrome, etc. then safety and legal liability becomes a concern.

The likelihood of leaching is not just a matter of whether the ingredients used to make a glaze are dangerous. The issue is complex, involving the ways in which the materials are prepared and fired and the formulations that are used. It is possible to use toxic materials safely and it is possible to compromise an otherwise safe glaze by unbalanced mixtures.

If a customer claims injury from leaching of your ware you have to demonstrate that there was no reason for you to have been concerned about the hazard and that you were diligent in researching the subject. If you don't know how to appraise a glaze's safety then play it safe. For example, there are ways to use barium safely but if you don't know them then don't use barium on food surfaces.

Is the glaze mature?

If a glaze is not properly melted one cannot expect it to be resistant to leaching. While a simple visual inspection of a glossy glaze is usually sufficient to judge the degree of melt, it is especially difficult to tell if a matte glaze is properly developed. This is because glazes can be matte because a network of surface crystals have developed, because the glaze has a surface texture imparted by incomplete mixing of oxides during the melt, because high alumina affects the reflectivity or index of refraction of the glass, or simply because the glaze is not melted.

If a glaze is not properly melted then it will be leachable. The simplest way to tell if this is the case is to fire the glaze at one and two cones higher and lower than your production temperature. Line up the samples and it should be obvious.

Is it balanced?

Glazes are leachable if they contain inadequate glass former and alumina. 'Flux saturated' glazes are very common because they develop interesting fired surfaces associated with non-homogeneous melts of more and less fluid components. However, for a glaze to be fluid, it needs to have lots of flux. If it has lots of flux then it is very likely that the silica and alumina are lacking. A glaze with high feldspar (50%+) is a classic example (feldspar by itself is leachable). If inadequate glass and intermediate oxides are available, coloring oxides that might otherwise be securely held in the glass structure may be available for leaching. Calculating the formula of your glaze (i.e. with INSIGHT) and comparing it with limit charts can be a good way to tell if adjustment is needed. Sometimes it is necessary to compromise a little of the visual character to produce a product more resistant to acid attack.

Another simple thing you can check for is material amounts that do not seem normal. It is common, for example, to see 5% talc in a glaze, but 30% is definitely not normal. Likewise more than 5% lithium carbonate or zinc is strange and needs explaining. Watch also for high amounts of Gerstley borate or boron frit (more than 10%) in high fire glazes, this is not normal. In addition, every glaze should have as much silica and kaolin as it can tolerate. High and middle temperature glazes with little or no silica or kaolin need an explanation. Low fire glazes must have lots of boron sourcing material like frit or they simply will not melt. Many frits are quite balanced as a low fire glaze (e.g. Ferro Frit 3195), others are not (e.g. Frit 3134) and need more added silica and kaolin.

Firing Temperature

Higher temperature glazes contain less flux and more silica and alumina. Since silica and alumina are so closely related to glaze stability it follows that high temperature glazes are intrinsicly more stable. However it is fairly easy to make unstable high temperature glazes also (fluid flux saturates are an example, they often contain little alumina). At high temperatures experimenters can mix a far greater range of materials and get a good melt because temperature is on their side. Thus it is easy to get 'sloppy' and adopt the attitude that if a glaze looks good it is also safe. Some potters even assume that any glaze is safe as long as it is fired at high temperature. It is common to see popular high fire recipes with very high metal oxide and barium contents. Matte glazes often contain abnormally large magnesia contents. These are destabilizing factors that temperature cannot counteract. With a knowledge of glaze chemistry you can create stable glazes at low fire, without it you can make unstable ones at high temperatures.

Does it contain known carcinogens or poisons?

If a glaze recipe contains materials that are 'surrounded in controversy' it might be best to eliminate or reduce these if they are not necessary. Barium for example, is used for the development of certain blue colors and its ability to produce a matte surface. However there is no justification for barium in a glaze having neither of these properties. The matte effects of barium can also be produced with calcia. Other materials that you should be careful about are manganese, copper (it increases glaze solubility), frits that you don't have an analysis for (may contain lead), chrome and lithia. There are others. Stains can contain a wide range of toxic metals, but they are optimized chemically to produce the intended color and therefore tend to contain less toxic metals than would be needed if you tried to produce the same color using raw metal oxides. In addition stains are smelted materials, they are mixtures of metals and stabilizers and are therefore inherently less soluble.

How do you apply on-glaze color on earthenware? Consider under-glaze.

If you apply pure stains or oxides on top of your glaze, there is a real danger than these might be soluble. It is best to mix metallic colors with a glaze (at least 50% glaze, but preferably a much higher glaze content). Do not mix on-glaze metallic colors with Gerstley Borate alone (it is soluble) or unbalanced frits (e.g. Ferro 3134), these needs much more alumina and silica to be stable. Putting color on the ware as a slip and applying a transparent glaze over top is the safest method for food surfaces. However if there is a danger of the overglaze crazing be careful about using extremely concentrated colored under slips since the cracks will expose them to the liquid the container holds. In addition an absorbent body with a crazed glaze will waterlog over time and the internal moisture will saturate with metals.

A liner glaze

The best solution is to use a liner glaze (see link to article on this) with no color on all surfaces that will be exposed to liquids. Liner glazes made from materials like kaolin, ball clay, bentonite, silica, feldspar, whiting, wollastonite, dolomite, nepheline syenite, Gerstley borate or boron frits (having only B2O3, Na2O, K2O, CaO, MgO, Al2O3, SiO2), talc, iron oxide, rutile, and zircon, titanium and tin opacifiers are relatively safe. Frits are also safe as long as you know that they contain oxides common to the above materials (no lead, barium). We have base glaze recipes available for low, medium and high temperatures (see link to "Concentrate on One Good Glaze" below). Be sure that colored under slips or glazes are not diffusing metals up into the liner glaze, especially where it might be thin. You can examine a broken cross section under a microscope to see if this is happening. If this is happening you will need to reduce the amount of flux in the colorant under layer.

Are your glazes crazing?

If your glazes craze and your ware is porous then there is a possibility you are creating a bacterial 'breeding ground'. If the craze lines are of adequate width then who knows what could live in there if the clay body supplies absorbed moisture from below. While there are many factors involved and this could be argued, we must admit that the greater body porosity, the wider the craze lines, and the less the ware is exposed to heat, the more this would be a threat. You can test if your ware is absorbing water by soaking it for a few days and putting an empty vessel in the microwave. If it gets hot (and it is not of a high iron clay or glaze) then it has absorbed water. Weighing a new piece before and after soaking will verify this. Remember also the matter of perception: Crazing dramatically weakens glazed ware. Over time it will lose its 'ring' and users will get the feeling that your ware is not good quality. As a result they may also question its other qualities, such as food safety.

Another factor to consider is this: Glazes craze because they have a high thermal expansion. Often high expansions are associated with low silica and alumina contents. Stability in glazes is almost always linked to the amount of silica and alumina, the more the better. Thus the crazing is often a tip-off that the glaze is potentially leachable.

Simple leaching tests you can do

All glass leaches to some extent when it comes into contact with acids or bases, especially if the contact occurs over a period of time or the acid is hot. This is evident by a change the gloss and texture of the glass surface over time. The ability of the glaze to pass two simple tests can be a good assurance that it will give trouble-free service.

These tests are not technical enough to guarantee that ware is going to be absolutely safe but they will certainly expose glazes that are obviously unsafe.

What to do if your glazes are soluble

If you find that your glazes are soluble, use ceramic calculations to increase the amount of silica and alumina and moderate the content of oxides that exist in inordinately large amounts. Test again to see if it worked. There is much information in the literature on this subject and often small changes that do not greatly impact the fired glass have significant effects of solubility.

The bottom line

Having your glaze lab-tested for metal release

Are you doing the simple tests? If not leave this till later. Please read the paragraph below before going this route. It is true that the only way to know for sure if your glaze is leaching is to have it tested at a credible lab. But think first about whether you able to interpret the results they give you? John Hesselberth, a potter who has made it his business in recent years to gather and evaluate information on limit formulas and glaze leaching, had this to say: 'You cannot predict leaching from limit formulas; although I believe a glaze within limits is more likely to be durable to leaching than one that is outside of limits--but being in limits is no guarantee.'See the links below or search for the term "toxicology" or "safety" on this site to find articles on specific materials (there are many).

List of Testing Labs

https://digitalfire.com/services/database.php?list=labs

Being Realistic About Have Leach-testing Done at a Lab

The idea of alot of people making leaching tests in isolation from each other and expecting to compare their results with some arbitrary standards to approve or deny a glaze is unrealistic. This is a science and requires standards and a history of testing data. If the vast majority of people have not done the simple things they can do to reduce the likelihood and evaluate glaze leaching, are they ready for the complicated tests? The real value of lab testing would come from relating many measurements taken over the years to glazes known to be more or less prone to leaching (by other types of testing and rationalization). Over time it would be evident which glazes were best, then the lab numbers of these could become a benchmark against which to compare others (with limitations realized by the experience). Are you ready for this?

Related Information

Copper can destabilize a glaze and make it soluble


This picture has its own page with more detail, click here to see it.

A closeup of a glossy Cone 6 glaze having 4% added copper carbonate. The bottom section has leached in lemon juice after 24 hours. This photo has been adjusted to spread the color gamut to highlight the difference. The leached section is now matte.

Black ash glaze for 20% raw metal pigments: Suitable for functional ware?


Saturated metal ash glaze

This picture has its own page with more detail, click here to see it.

This glaze is 49% Wood Ash, 24% Soda Feldspar and 27% Ball Clay. 10 copper carbonate and 10 manganese dioxide are added to that. This beautiful sculpture was made by Dan Ingersoll, aesthetically this glaze is perfect for it. But there are two red flags here. Significant manganese and copper metal fumes are certain to be generated at cone 10 (they are seriously not healthy) so anyone using this must be very careful. But there is something much more serious - this glaze is being used on functional ware. Copper is well known to destabilize other metals in the fired glass. This 10:10 combination is a perfect storm for leaching heavy metal into food and drink. This is not an argument for the use of commercial glazes, it is one for common sense application of the concept of limit recipes.

Commercial glazes on decorative surfaces

Your own on food surfaces


This picture has its own page with more detail, click here to see it.

These cone 6 porcelain mugs are hybrid. Three coats of a commercial glaze painted on the outside (Amaco PC-30) and my own liner glaze, G2926B, poured in and out on the inside. When commercial glazes (made by one company) fit a stoneware or porcelain (made by another company) it is by accident, neither company designed for the other! For inside food surfaces make or mix a liner glaze already proven to fit your clay body, one that sanity-checks well (as a dipping glaze or a brushing glaze). In your own recipes you can use quality materials that you know deliver no toxic compounds to the glass and that are proportioned to deliver a balanced chemistry. Read and watch our liner glazing step-by-step and liner glazing video for details on how to make glazes meet at the rim like this.

If you think one slip fits any body, think again


This picture has its own page with more detail, click here to see it.

This flake shivered off the rim of a low fire terra cotta mug. It is Fishsauce slip. It is about 2 inches long and has razor sharp edges. This is not the sort of thing you would want to be falling into your coffee or food and then eating! This flake did give evidence that it was loosening so there was little danger of me consuming it, but smaller flakes can go unnoticed. Slips (or engobes) must be drying compatible, have the same firing shrinkage, the same thermal expansion and be quartz inversion compatible with the body. It is easy to ignore all that and pretend that it works, but the bond between engobe and body is fragile at low fire and easily compromised by the above incompatibilities. Slips must be fitted to the specific body, glaze and temperature; that involves a testing program and often a little chemistry. I have documented online how to I adapted this slip to Plainsman Terrastone 2 using my account at insight-live.com.

Liner glaze is coffee-staining and leaching after two years. Is it toxic?


The white inside of a mug is coffee-staining

This picture has its own page with more detail, click here to see it.

This is a cone 04 terra cotta piece. The coffee stain cannot be removed because the coffee has also leached off the surface gloss. Glazes are glass. Glass is leachable if the chemistry is out-of-balance. So is this glaze poisoning the user? No, it has an insurance policy. It is transparent, made from a mix of two frits (Ferro 3124, 3134) plus kaolin and silica. The recipe contains no heavy metal colorants or pigments and no toxic fluxes like lithium or barium. But the body is red, how can the glaze be white? A white porcelain-like engobe layer was applied at the leather hard stage and it was clear-glazed after bisque. The fix: The predominant frit, 3134, has almost no Al2O3 (the oxide most important in producing durability). So I increased the Al2O3 (doing the chemistry in my Insight-live.com account). I also began firing one cone higher, at cone 03.

Metal leaching from ceramic glazes: Lab report example and a better way


Metal leaching from ceramic glazes: Lab report example

This picture has its own page with more detail, click here to see it.

This lab is certified by the US Department of Environmental Protection (DEP) for drinking water and wastewater analysis. They also provide pottery glaze leaching analyses (an acid solution is kept in contact with the glaze and then analysed for trace levels of specific metals). Each suspected metal to be tested for entails a separate charge ($30-60 in this case, could be less for you). That means that testing one glaze for several metals could cost $200. How to make sense of these numbers? Google the term: "heavy metals drinking water standards", and click "Images" to find charts with lots of data. Searching pages for this term will find books having detailed sections on each of the metals. Typically you are only interested in one metal in a specific glaze (often cobalt or manganese). There are ways to sleep better (about the likelihood your glazes are leaching metals) if you cannot do this: Do a simple GLLE test. And avoid online trafficking in hazardous recipes. Better to find a quality base glaze (matte and transparent) that works well on your clay body. Then add colorants, opacifiers and variegators; but doing so in a conservative manner. And use a liner glaze on food surfaces.

Why would I use a heavily pigmented black glaze on a food surface?


Two mugs, black glaze on the inside, red glaze on the outside

This picture has its own page with more detail, click here to see it.

These are actually two different cone 6 base glazes to which I add a black stain. I trust them because I know what is in them, I formulated and perfected them myself: G2926B clear and GA6-B Alberta Slip base. They are durable, fit my clay bodies, melt well yet can host a stain without loss of gloss. I even know the chemistry, both have plenty of SiO2 and Al2O3, that is a hallmark of durability. I fired these using the PLC6DS schedule. I add 5% black stain to the former and 4% to the latter, both yield a jet-black. The GA6-B requires ball milling. Stains are inherently much safer to use than raw metal oxide colorants because they are sintered as colorant/stabilizer blends. And much less is needed. Contrast that with raw metal oxides, it is common to find black recipes containing up to 15% of blends of nickel, cobalt, iron and manganese! At times the manganese alone can be 8% or more! So, I feel relatively safe using these coloured glazes on a surface that will be exposed to hot and acidic liquids.

It is possible to spot a leaching glaze just by looking at it!


A matte black coffee mug with leaching glaze

This picture has its own page with more detail, click here to see it.

This glaze looks too matte, too metallic, too crystalline. This picture was sent to me by a worried person who had bought it and noticed it discolouring on the inside. The potter may very well have considered this safe just because it was fired to cone 10. It is common among potters to overload glazes with raw metal oxide blends, often 15% or more (e.g. manganese, copper, iron, nickel, cobalt). These percentages cannot be held in solution in the melt as it cools and solidifies, so they precipitate out and crystallize, especially if the glaze is not melting well or has insufficient SiO2. The crystalline forms of these metals might look nice to some people, but the glaze is likely to leach them. It is better to use a ceramic stain to create a black like this, adding it to a stable matte base glaze (one that melts well and has sufficient SiO2 and Al2O3 to create a durable glass). The concept of a limit recipe is helpful in eyeballing recipes for their likelihood of leaching.

Two black cone 6 glazes recipes. One leaches metals. Why?


Black-glazed sample tiles showing leaching

This picture has its own page with more detail, click here to see it.

We tested susceptibility to leaching of a stained glaze (top two) and another colored with raw metal oxides (bottom two) using the GLLE test (they were left overnight in vinegar and lemon juice). All the samples were fired using the C6DHSC firing schedule. The top two are G3914A (GA6-B Alberta Slip base with an addition of only 4% Mason 6600 black stain). There is no sign of leaching (Drano and bleach likewise did not affect it). The bottom two are G2926B transparent with 10% manganese dioxide and 5% copper oxide added (a common way to get black). The G2926B transparent base is proven, its surface shows no signs of gloss-loss in any testing we have done. But with manganese and copper added it is a very different story. Not only was this not nearly as black, but the vinegar and lemon juice matted and blued the top sections. Obviously, a ceramic stain added to the Alberta Slip GA6-B base is a far better way to make a leach-resistant black. Is it better than adding the black stain to G2926B? Yes, because far less is needed since the GA6-B base already has plenty of pigmentation.

Links

Articles Having Your Glaze Tested for Toxic Metal Release
Having Your Glaze Tested for Metal Release
Articles An Overview of Ceramic Stains
Understanding the advantages of disadvantages of stains vs. oxide colors is the key to choosing the best approach
Articles Attack on Glass: Corrosion Attack Mechanisms
Max Richens outlines the various mechanisms by which acids and bases can dissolve glass and glazes. He provides some information on stabilizing glazes against attack.
Articles Crazing and Bacteria: Is There a Hazard?
A post to a discussion on the clayart group by Gavin Stairs regarding the food safety of crazed ware.
Articles Is Your Fired Ware Safe?
Glazed ware can be a safety hazard to end users because it may leach metals into food and drink, it could harbor bacteria and it could flake of in knife-edged pieces.
Articles Leaching Cone 6 Glaze Case Study
An example of how we can use INSIGHT software to determine of a glaze is likely to leach
Articles Concentrate on One Good Glaze
It is better to understand and have control of one good base glaze than be at the mercy of dozens of imported recipes that do not work. There is a lot more to being a good glaze than fired appearance.
Tests Glaze Leaching Test
Simple tests to evaluate the stability of a ceramic or pottery glaze against leaching metals in food or drink.
Troubles Glaze Crazing
Ask the right questions to analyse the real cause of glaze crazing. Do not just treat the symptoms, the real cause is thermal expansion mismatch with the body.
Hazards Overview of Material Safety by Gavin Stairs
Toxicology and ceramic materials is a complex subject, what materials and methods pose the greatest dangers, which are the safest?
Hazards Copper Oxide and Carbonate
Materials Feldspar
In ceramics, feldspars are used in glazes and clay bodies. They vitrify stonewares and porcelains. They supply KNaO flux to glazes to help them melt.
Glossary Leaching
Ceramic glazes can leach heavy metals into food and drink. This subject is not complex, there are many things anyone can do to deal with this issue
Glossary Toxicity
Common sense can be applied to the safe use of ceramic materials. The obvious dangers are breathing the dust and inhaling the fumes they produce during firing. Here is a round-up of various materials and their obvious hazards.
Oxides Sm2O3 -
Typecodes Ceramic Testing Labs

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy