A ChatBot gives jaw-dropping glaze recipe advice - Jan 2025
A Low Cost Tester of Glaze Melt Fluidity
A One-speed Lab or Studio Slurry Mixer
A Textbook Cone 6 Matte Glaze With Problems
Adjusting Glaze Expansion by Calculation to Solve Shivering
Alberta Slip, 20 Years of Substitution for Albany Slip
An Overview of Ceramic Stains
Are You in Control of Your Production Process?
Are Your Glazes Food Safe or are They Leachable?
Attack on Glass: Corrosion Attack Mechanisms
Ball Milling Glazes, Bodies, Engobes
Binders for Ceramic Bodies
Bringing Out the Big Guns in Craze Control: MgO (G1215U)
Can We Help You Fix a Specific Problem?
Ceramic Glazes Today
Ceramic Material Nomenclature
Ceramic Tile Clay Body Formulation
Changing Our View of Glazes
Chemistry vs. Matrix Blending to Create Glazes from Native Materials
Concentrate on One Good Glaze
Converting between Oxide Weight %, Mole % and Unity Formula
Copper Red Glazes
Crazing and Bacteria: Is There a Hazard?
Crazing in Stoneware Glazes: Treating the Causes, Not the Symptoms
Creating a Non-Glaze Ceramic Slip or Engobe
Creating Your Own Budget Glaze
Crystal Glazes: Understanding the Process and Materials
Deflocculants: A Detailed Overview
Demonstrating Glaze Fit Issues to Students
Diagnosing a Casting Problem at a Sanitaryware Plant
Drying Ceramics Without Cracks
Duplicating Albany Slip
Duplicating AP Green Fireclay
Electric Hobby Kilns: What You Need to Know
Fighting the Glaze Dragon
Firing Clay Test Bars
Firing: What Happens to Ceramic Ware in a Firing Kiln
First You See It Then You Don't: Raku Glaze Stability
Fixing a glaze that does not stay in suspension
Formulating a body using clays native to your area
Formulating a Clear Glaze Compatible with Chrome-Tin Stains
Formulating a Porcelain
Formulating Ash and Native-Material Glazes
G1214M Cone 5-7 20x5 glossy transparent glaze
G1214W Cone 6 transparent glaze
G1214Z Cone 6 matte glaze
G1916M Cone 06-04 transparent glaze
Getting the Glaze Color You Want: Working With Stains
Glaze and Body Pigments and Stains in the Ceramic Tile Industry
Glaze chemistry using a frit of approximate analysis
Glaze Recipes: Formulate and Make Your Own Instead
Glaze Types, Formulation and Application in the Tile Industry
Having Your Glaze Tested for Toxic Metal Release
High Gloss Glazes
Hire Us for a 3D Printing Project
How a Material Chemical Analysis is Done
How desktop INSIGHT Deals With Unity, LOI and Formula Weight
How to Find and Test Your Own Native Clays
I have always done it this way!
Inkjet Decoration of Ceramic Tiles
Is Your Fired Ware Safe?
Leaching Cone 6 Glaze Case Study
Limit Formulas and Target Formulas
Low Budget Testing of Ceramic Glazes
Make Your Own Ball Mill Stand
Making Glaze Testing Cones
Monoporosa or Single Fired Wall Tiles
Organic Matter in Clays: Detailed Overview
Outdoor Weather Resistant Ceramics
Painting Glazes Rather Than Dipping or Spraying
Particle Size Distribution of Ceramic Powders
Porcelain Tile, Vitrified Tile
Rationalizing Conflicting Opinions About Plasticity
Ravenscrag Slip is Born
Recylcing Scrap Clay
Reducing the Firing Temperature of a Glaze From Cone 10 to 6
Setting up a Clay Testing Program in Your Company or Studio
Simple Physical Testing of Clays
Single Fire Glazing
Soluble Salts in Minerals: Detailed Overview
Some Keys to Dealing With Firing Cracks
Stoneware Casting Body Recipes
Studio Management Software 2026 (booking)
Substituting Cornwall Stone
Super-Refined Terra Sigillata
The Chemistry, Physics and Manufacturing of Glaze Frits
The Effect of Glaze Fit on Fired Ware Strength
The Four Levels on Which to View Ceramic Glazes
The Majolica Earthenware Process
The Potter's Prayer
The Right Chemistry for a Cone 6 Magnesia Matte
The Trials of Being the Only Technical Person in the Club
The Whining Stops Here: A Realistic Look at Clay Bodies
Those Unlabelled Bags and Buckets
Tiles and Mosaics for Potters
Toxicity of Firebricks Used in Ovens
Trafficking in Glaze Recipes
Understanding Ceramic Materials
Understanding Ceramic Oxides
Understanding Glaze Slurry Properties
Understanding the Deflocculation Process in Slip Casting
Understanding the Terra Cotta Slip Casting Recipes In North America
Understanding Thermal Expansion in Ceramic Glazes
Unwanted Crystallization in a Cone 6 Glaze
Using Dextrin, Glycerine and CMC Gum together
Volcanic Ash
What Determines a Glaze's Firing Temperature?
What is a Mole, Checking Out the Mole
What is the Glaze Dragon?
Where do I start in understanding glazes?
Why Textbook Glazes Are So Difficult
Working with children

Creating a Non-Glaze Ceramic Slip or Engobe

Description

It can be difficult to find an engobe that is drying and firing compatible with your body. It is better to understand, formulate and tune your own slip to your own body, glaze and process.

Article

Non-glaze slips (referred to as engobes when applied thickly) for pottery and tile decoration have long fostered great fascination. Almost everyone has marvelled at the simple beauty of terra cotta ware decorated with white slip and finished with a transparent glaze. Many potters are adapting this age old process to stoneware and porcelain. Industry, especially tile, routinely applies slips and engobes (e.g. white layers are put on darker burning dry tiles before applying glaze over top). They are almost universally used in the single fire process. This is logical since their key application is to cover over dark burning or dirty bodies made from local materials, in these cost conscious situations it makes little sense to fire more times than needed.

Pairing of engobe-thickness slips with a specific body is difficult so recipes travel even less well than glazes. They need to be drying, firing and thermal expansion compatible with both the underlying body and overlying glaze. Each of these should be tested individually. Compare this to a glaze being applied directly to a bisque body: you only need to focus on thermal expansion compatibility with the body; this is so much easier.

Consider the first major challenge: Adhesion with the body (both in drying and firing), getting the stuff to stick on! If the slip is applied thick enough and does not shrink at the correct rate or amount during drying and firing, cracks will develop or it will flake off. No matter what logic, theory or lab instruments might indicate or what others might advise, if cracking or flaking is occurring it is much more likely you need to react by adjusting the recipe appropriately than by adjusting the way it is prepared or applied. Different factors are involved in attaining compatibility for firing and drying and a change that improves one aspect of fitness may detrimentally affect another. While each material in the recipe is there for a drying, firing, adhesion, thermal expansion or aesthetic reason, it is also potentially detrimental to one or more other parts of the process; this means developing the right recipe is a real juggling act.

The most obvious use of a fine-grained white engobe is to cover a dark colored (and possibly coarse-grained) body so that brightly colored or lightly shaded glazes appear as they do on fine porcelain. The tile industry is by far the largest user of engobes, it is very common for them to use red burning clays (they are often locally available and fire much stronger than light burning clays at low temperatures). They cover the red bodies with a white burning opaque engobe. Obviously good adherence to the fired body is paramount, so the engobe needs frit or other melters to create a glass bond. Adherence will obviously be best on vitrified bodies where an interface can develop (if the body does not vitrify well extra frit will be needed to create a more glassy interface, but not so much that opacity is lost).

Dry Adherence, Shrinkage, Hardness; Slurry Suspension

Fired Shrinkage and Adherence

The fired interface between slip and body will never be as good as one between glaze and body. This is potentially a weakness if the fired adherence of the slip is not evaluated and optimized. Since slips do not melt formulation is normally done on the recipe level (the physical properties must simply be observed, ceramic calculations are not really applicable).

Thermal Expansion

Laydown and Application

You need a different mindset than with glazes to have success with engobes. Glazes smooth out when they melt, engobes do not. Like paint, the surface you apply is the one you get after firing. Thus drips, variations in thickness, roughness, pinholes, bubbles, etc are going to show. Normally a glaze over-layer is not going to be thick enough to cover over problems in the slip laydown, infact, slip irregularities can produce glaze defects. Application for tiles is straightforward since the surface is flat and horizontal, but for uneven shapes it is a lot more complicated. Here are some ideas.

The Recipe

Conceptually a recipe can be as simple as a porcelain body with enough added frit for adherence but no so much that glass development reduces the opacity. This can be a fine line. For example, only 15% Ferro Frit 3134 may flux it too much at cone 04. It is better to mix your slip as a recipe of ingredients that include those for the porcelain rather than just adding something to a powdered porcelain whose recipe you do not know, this will give you the needed flexibility to adjust.

For high temperature you should be able to flux using feldspar and other raw materials rather than frits (e.g. wollastonite, dolomite). Thus, an alteration of the standard 25 porcelain could be the 40% kaolin, 35% feldspar, 25% silica (I have combined the ball clay and kaolin to just kaolin (for extra whiteness), you may need to add a plasticizer like Veegum. If it can be more mature, try 40 feldspar at the expense of silica this time. For medium temperature a typical base porcelain recipe might be 40 kaolin/ball clay, 40 feldspar and 20 silica. Add 5% of a boron frit (like Ferro 3134). The idea is to tune it degree of maturity to get maximum melting without loss of opacity.

For more whiteness consider using a whiter kaolin or adding some zircopax (perhaps 5%, for opacity). If the slip is too plastic, use calcined kaolin for part of the clay complement if needed to cut drying shrinkage. If it is flaking off, then try adding Veegum (up to 10%). And as a last resort use gum to harden it and give better flow (however it is better to adjust or substitute clays to get the flow and drying properties needed, gummed slips dry slower).

A Few General Notes About Using Slip

Creating your own slip will take time, determination, and a methodical approach with plenty of adapting over time. Like glazes, it is far better to have one recipe you understand and control than mess around with 10 that you don't understand and don't work?

Related Information

Applying an engobe by pouring or spraying


This picture has its own page with more detail, click here to see it.

An example of an engobe (slip) applied to dry ware and then fired at cone 2. The one of the left has been poured, the right sprayed. Control of the thickness of engobes is important, thus the specific gravity and viscosity of the slurries are very important. Engobes are invaluable since a red or brown burning body can be made to fire white like porcelain (enabling much better glaze surface quality).

An extreme case of firing shrinkage mismatch between engobe and body


This picture has its own page with more detail, click here to see it.

Example of fritted white engobe over-fired to cone 2. During firing it has shrunk and the bond with the body has been completely compromised. The body has a firing shrinkage of about 6% but the slip is closer to 10%. Because glazes melt they do not have a firing shrinkage. But engobes do and it must be compatible with the body.

Here’s why engobes shouldn’t melt

And also why they needn't contain zircon


An over mature engobe is not opaque

This picture has its own page with more detail, click here to see it.

Since white burning slips are made from refractory materials they are not nearly as vitreous as terracotta bodies, they need help to mature and a frit is the natural answer. With the right amount, fired shrinkage can be matched to the body while the slip remains opaque.

L3685A slip on the left: An adjustment to the popular "Fish Sauce" recipe (which is basically a super plastic white body). 8% Frit 3110 replaces 8% Pyrax to make it glass-bond to the body better while remaining completely opaque.

Right L3685C: It has 15% frit, moving it into glaze territory, with translucency replacing opacity. Although expensive zircon could be added to restore opacity, that doesn’t fix the excessive firing shrinkage it now has, mismatching it with the body (which becomes more eventful the thicker it is applied).

Bi-Clay strips test compatibility between engobe and body


This picture has its own page with more detail, click here to see it.

Slips and engobes are fool-proof, right? Just mix the recipe you found on the internet, or that someone else recommends, and you are good to go. Wrong! Low fire slips need to be compatible with the body in two principle ways: drying and firing. Terra cotta bodies have low shrinkage at cone 06-04 (but high at cone 02). The percentage of frit in the engobe determines its firing shrinkage at each of those temperatures. Too much and the engobe is stretched on, too little and it is under compression. The lower the frit the less the glass-bonding with the body and the more chance of flaking if they do fit well (either during the firing or after the customer stresses your product). The engobe also needs to shrink with the body during drying. How can you measure compatibility? Bi-body strips. First I prepare a plastic sample of the engobe. Then I roll 4 mm thick slabs of it and the body, lay them face-to-face and roll that down to 4 mm again. I cut 2.5x12 cm bars and dry and fire them. The curling indicates misfit. This engobe needs more plastic clay (so it dry-shrinks more) and less frit (to shrink less on firing).

Solving a difficult engobe flaking problem


This picture has its own page with more detail, click here to see it.

This demonstrates the difficulty you can encounter when trying to get an engobe working with a clay body. Here the slip/glaze is flaking off the rim of pieces at cone 04 (does not happen at 06). The front bi-clay bar demonstrates the white and red clays dry well together (the slight curve happened on the drying). They also fire well together (the curvature did not change on firing). The back two thin bars seem to demonstrate thermal expansion compatibility: a thick layer of glaze is not under enough compression to curve either bar during firing. While the white clay contains 15% frit and forms a good bond with the red body, that bond is not nearly as good as the one between the glaze and the white slip. Yet it is still flaking off the rim at the slip/body interface. Why? At first it seemed that failure was happening at quartz inversion (because the body had less quartz than the white slip). However now it appears that the combination of compressions of the slip and glaze are sufficient to break the slip-body bond on concave contours. The compression of the slip and glaze likely did not demonstrate well on the bars because at this low a temperature they are not vitreous enough to be easily curled.

How stop dripping and running:

Add water! Then make it thixotropic.


This picture has its own page with more detail, click here to see it.

The white slip on the left, L3685Z2, (applied to a leather hard cup) is dripping downward from the rim (even though it was held upside down for a couple of minutes!). Yet that slurry was very viscous with a 1.48 specific gravity. Why? Because it was not thixotropic. The fix? I watered it down to 1.46 (making it runny) and added pinches of powdered Epsom salts (while mixing vigorously) until it thickened enough to stop motion in about 1-2 seconds on mixer shut-off. But that stop-motion is followed by a bounce-back. That is the thixotropy. It is easy to overdo the Epsom salts (gelling it too much), I add a drop or two of Darvan to rethin it if needed. When the engobe is right, it gels after about 10 seconds of sitting, so I can stir it, dip and extract the mug, shake to drain it and then it gels and holds in place. Keep in mind, this is a pottery project. In industry, they deflocculate engobes to reduce water content and then impose thixotropy, but that is more technical than the average potter would want.

The same engobe. Same water content. What is the difference?


Two samples, the same engobe runs but not the other

This picture has its own page with more detail, click here to see it.

The engobe on the left, even though it has a fairly low water content, is running off the leather hard clay, dripping and drying slowly. The one on the right has been flocculated with epsom salts (powdered), giving it thixotropy (ability to gel when not in motion but flow when in motion). Now there are no drips, there are no thin or thick sections. It gels after a few seconds and can be uprighted and set on the shelf for drying.

Creating a Body/slip Equilibrium in Terra Cotta Ware


This picture has its own page with more detail, click here to see it.

L3685X white slip (left mug) has 5% more frit than Y (right). The frit is a melter, creating more glass bonds to adhere it to the body (it also hardens it and darkens the color a little). But the frit also increases firing shrinkage, 'stretching' the white layer on the body as the kiln cools (the slightly curled bi-clay bar demonstrates that). However the glaze, G2931G, is under some compression (to prevent crazing), it is therefore 'pushing back' on the white slip. This creates a state of equilibrium. The Y slip on the right is outside the equilibrium, it flakes off at the rim because the bond is not good enough. Adding more frit, the other side of the balance, would put the slip under excessive tension, reducing ware strength and increasing failure on exposure to thermal shock (the very curled bi-clay bar in the front, not this clay/slip demonstrates the tension a poorly fitted slip could impose).

A reason for DIY underglazes:

Glass-bonding with the body instead of just seeking color


Orange underglaze is flaking off

This picture has its own page with more detail, click here to see it.

This flaking is happening at the interface between the body and orange commercial underglaze (the firing is cone 05). The reason is simple.

Pure stains contribute only one ceramic property: Color! Commercial underglazes sold in jars dilute stains into a recipe of materials, a powder medium, designed to impart the missing properties. However, suppliers like to quote products as suitable over a wide range (e.g. cone 06-6). Of course, at cone 06, they have almost no glass development for bonding to the body and at cone 6 they may well be melted. In this case, the stain used is refractory and a high percentage is needed. So the bond with the body is very poor. A thick layer coupled with an incompatible thermal expansion can make the underglaze/glaze layer pop right off.

Is a DIY version possible? Imagine if you created a powder medium (e.g. L3685Z3) containing enough frit to counter the refractory character of the stain and develop the needed glass to bond with the body. That would solve this problem.

Michael Cardew might be turning over in his grave!


Michael Cardew Pioneer Pottery book

This picture has its own page with more detail, click here to see it.

This post got a lot of negative reaction on social media. To be clear, I work both sides of the fence, making my living on selling prepared glazes and clay bodies but I get my satisfaction being closer to the materials and processes. That is what enables me to give customer support. I am not an artist, ceramic art is outside the scope of this page. For part of my life in the craft of pottery I am also guilty of what I lament below. In all my years dealing with customer traffic at our store I have never once had a customer that was offended by seeing new clay and glaze recipes we are discovering in the studio and lab, that are better and cheaper than prepared ones. But online some are somehow offended by what follows. 80 manufacturers are selling convenience and encouraging disconnection - although I work for one of them I am a voice of caution about this.

This book was once a “Bible” of hobby and professional potters. They were independent and resourceful. They made their own clays and glazes, knew the materials, built their own kilns. Now we scan social media sites for ideas on layering expensive prepared goopy brushing glazes and hope they melt together into something presentable. Many have even forgotten how to wedge clay properly. We describe processes using mystical art language and exchange likes and poor advice on social media. Those who still know how to retotal a recipe and venture into mixing their own often end up in the online trafficking of an endless parade of recipes that don’t work. Now we even outsource design to AI. Even Nigeria, the very country about whom Cardew wrote, has lost its pottery tradition.

I never appreciated the book back there. Even though he came to visit us in 1973. I have always just taken whatever clay I needed out of our warehouse, but now that I very often make my own clay it really resonates. I got this copy on eBay, I value it as an inspiration to be more closely connected with the planet and the minerals it gifts us (of course I would not do everything as he does). He was no dinosaur, he understood and taught glaze chemistry and material mineralogy, his work was the basis for many prepared glazes we buy today. "Progress" is defined by some as convenience products that make modern ceramics easy. But I believe that, for many, progress is arming yourself with a little more understanding - it enables making better quality ware, in less time, for less expense and time than with prepared products.

Links

Materials Ravenscrag Slip
A light-colored silty clay that melts to a clear glaze at cone 10R, with a frit addition it creates a good base for a wide range of cone 6 glazes.
Articles Ravenscrag Slip is Born
The story of how Ravenscrag Slip was discovered and developed might help you to recognize the potential in clays that you have access to.
Troubles Crawling
Crawling glazes pull into islands, leaving bare spots on the body. Asking yourself the right questions will surface the real cause and help you deal with the problem, not the symptoms.
Glossary Ceramic Slip
The term Slip can have various meanings in traditional ceramics.
Glossary Once-Fire
The practice of once-firing ceramics (no bisque) to produce fully glazed products. Considerable technical expertise and good testing are required to make it work. This is not a shortcut to skipping bisque firing.
Glossary Mocha glazes
A technique used by ceramic artists to decorate pottery. It happens when bleeding occurs at the edges of a thin colored acidic mixture painted over a still-wet slip.
Glossary Brushing Glaze
Hobbyists and increasing numbers of potters use commercial paint-on glazes. It's convenient, there are lots of visual effects. There are also issues compared to dipping glazes. You can also make your own.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy