This is modelled after the C6DHSC firing schedule. Please read its notes to understand the logic.
| Step | °C | °F | Hold | Time | |
|---|---|---|---|---|---|
| 1 | 60°C/hr to 104C | 108°F/hr to 220F | 60min | 2:20 | |
| 2 | 194°C/hr to 1128C | 350°F/hr to 2063F | 10min | 7:46 | |
| 3 | 60°C/hr to 1183C | 108°F/hr to 2163F | 10min | 8:52 | |
| 4 | 500°C/hr to 1128C | 900°F/hr to 2063F | 30min | 9:28 | |
| 5 | 83°C/hr to 760C | 150°F/hr to 1400F | 13:53 |
| Firing Schedules |
Plainsman Cone 6 Drop-and-hold, Slow Cool
350F/hr to 2100F, 108/hr to 2200, hold 10 minutes, fastdrop to 2100, hold 30 minutes, 150/hr to 1400 |
| Firing Schedules |
Bartlett Fast Glaze Cone 6
570F/hr to 1982F, 200/hr to 2232, no holds, no control cool |
| Firing Schedules |
Mastering Glazes Cone 6
Six-step with controlled drops to 1000C and 760C |