Material | Amount |
---|---|
Ferro Frit 3110 | 50.00 |
Zinc Oxide | 22.00 |
Silica | 25.00 |
Lithium Carbonate | 3.00 |
Added | |
Titanium | 2.00 |
102.00 |
This was fired first on a body having 38 silica, 28.5 ball clay, 28.5 nepheline and 5 bentonite (L3659B). There is no crazing at all but also no crystallization.
The firing was 750F/hr to cone 6, 750F to 1800F and soak for 4 hours.
Cone 6 crystalline glaze on L3659B body, there is no crazing.