A ChatBot gives jaw-dropping glaze recipe advice - Jan 2025A Low Cost Tester of Glaze Melt FluidityA One-speed Lab or Studio Slurry MixerA Textbook Cone 6 Matte Glaze With ProblemsAdjusting Glaze Expansion by Calculation to Solve ShiveringAlberta Slip, 20 Years of Substitution for Albany SlipAn Overview of Ceramic StainsAre You in Control of Your Production Process?Are Your Glazes Food Safe or are They Leachable?Attack on Glass: Corrosion Attack MechanismsBall Milling Glazes, Bodies, EngobesBinders for Ceramic BodiesBringing Out the Big Guns in Craze Control: MgO (G1215U)Can We Help You Fix a Specific Problem?Ceramic Glazes TodayCeramic Material NomenclatureCeramic Tile Clay Body FormulationChanging Our View of GlazesChemistry vs. Matrix Blending to Create Glazes from Native MaterialsConcentrate on One Good GlazeConverting between Oxide Weight %, Mole % and Unity FormulaCopper Red GlazesCrazing and Bacteria: Is There a Hazard?Crazing in Stoneware Glazes: Treating the Causes, Not the SymptomsCreating a Non-Glaze Ceramic Slip or EngobeCreating Your Own Budget GlazeCrystal Glazes: Understanding the Process and MaterialsDeflocculants: A Detailed OverviewDemonstrating Glaze Fit Issues to StudentsDiagnosing a Casting Problem at a Sanitaryware PlantDrying Ceramics Without CracksDuplicating Albany SlipDuplicating AP Green FireclayElectric Hobby Kilns: What You Need to KnowFighting the Glaze DragonFiring Clay Test BarsFiring: What Happens to Ceramic Ware in a Firing KilnFirst You See It Then You Don't: Raku Glaze StabilityFixing a glaze that does not stay in suspensionFormulating a body using clays native to your areaFormulating a Clear Glaze Compatible with Chrome-Tin StainsFormulating a PorcelainFormulating Ash and Native-Material GlazesG1214M Cone 5-7 20x5 glossy transparent glazeG1214W Cone 6 transparent glazeG1214Z Cone 6 matte glazeG1916M Cone 06-04 transparent glazeGetting the Glaze Color You Want: Working With StainsGlaze and Body Pigments and Stains in the Ceramic Tile IndustryGlaze chemistry using a frit of approximate analysisGlaze Recipes: Formulate and Make Your Own InsteadGlaze Types, Formulation and Application in the Tile IndustryHaving Your Glaze Tested for Toxic Metal ReleaseHigh Gloss GlazesHire Us for a 3D Printing ProjectHow a Material Chemical Analysis is DoneHow desktop INSIGHT Deals With Unity, LOI and Formula WeightHow to Find and Test Your Own Native ClaysI have always done it this way!Inkjet Decoration of Ceramic TilesIs Your Fired Ware Safe?Leaching Cone 6 Glaze Case StudyLimit Formulas and Target FormulasLow Budget Testing of Ceramic GlazesMake Your Own Ball Mill StandMaking Glaze Testing ConesMonoporosa or Single Fired Wall TilesOrganic Matter in Clays: Detailed OverviewOutdoor Weather Resistant CeramicsPainting Glazes Rather Than Dipping or SprayingParticle Size Distribution of Ceramic PowdersPorcelain Tile, Vitrified TileRationalizing Conflicting Opinions About PlasticityRavenscrag Slip is BornRecylcing Scrap ClayReducing the Firing Temperature of a Glaze From Cone 10 to 6Setting up a Clay Testing Program in Your Company or StudioSimple Physical Testing of ClaysSingle Fire GlazingSoluble Salts in Minerals: Detailed OverviewSome Keys to Dealing With Firing CracksStoneware Casting Body RecipesStudio Management Software 2026 (booking)Substituting Cornwall StoneSuper-Refined Terra SigillataThe Chemistry, Physics and Manufacturing of Glaze FritsThe Effect of Glaze Fit on Fired Ware StrengthThe Four Levels on Which to View Ceramic GlazesThe Majolica Earthenware ProcessThe Potter's PrayerThe Right Chemistry for a Cone 6 Magnesia MatteThe Trials of Being the Only Technical Person in the ClubThe Whining Stops Here: A Realistic Look at Clay BodiesThose Unlabelled Bags and BucketsTiles and Mosaics for PottersToxicity of Firebricks Used in OvensTrafficking in Glaze RecipesUnderstanding Ceramic MaterialsUnderstanding Ceramic OxidesUnderstanding Glaze Slurry PropertiesUnderstanding the Deflocculation Process in Slip CastingUnderstanding the Terra Cotta Slip Casting Recipes In North AmericaUnderstanding Thermal Expansion in Ceramic GlazesUnwanted Crystallization in a Cone 6 GlazeUsing Dextrin, Glycerine and CMC Gum togetherVolcanic AshWhat Determines a Glaze's Firing Temperature?What is a Mole, Checking Out the MoleWhat is the Glaze Dragon?Where do I start in understanding glazes?Why Textbook Glazes Are So DifficultWorking with children
Understanding Ceramic Oxides
Description
Fired glazes are composed of oxide building blocks. Each of the oxides contributes different properties to the fired glaze and interacts with others in different ways. Understanding these gives you control.
Article
The ancient Chinese thought of glazes as being made of bones, flesh, and blood. They were very perceptive! The silica content of a glaze acts like a framework, the alumina acts to give it body, and the fluxes melt it and impart character acting as the lifeblood.
In understanding fired properties, it is helpful to view materials as sources of oxides. However, remember that although it is chemically possible to supply a given oxide from many materials, often other factors make one of them preferable. For example, kaolin is an ideal source of alumina since it also imparts suspension and hardening properties to the glaze slurry.
Following is a list of the major oxides. There are a multitude of textbooks with more information on this subject. However, the data is widely scattered and thus difficult to study. The best source of information is the oxides area on this website.Not only is each oxide described in detail but properties are assigned so that it can be searched by category. For example, if you need to produce purple you can look up the 'purple' property area and see a list of all the chemistries that produce it.
Major Oxides
- SiO2 - Silicon dioxide is supplied by silica, feldspar, and kaolin. It is the principle glass forming oxide and normally comprises more than 60% of most glazes and clays. It has a low expansion and high melting temperature.
- Al2O3 - Aluminum oxide is supplied by kaolin and feldspar. It combines well with silica and basic oxides to give body, durability, and stability to glazes. It has a low expansion and high melting temperature.
- B2O3 - Boric oxide is supplied by borax frits, gerstley borate, (or colemanite). It is a low temperature low expansion equivalent of silica.
- CaO - Calcium oxide is supplied by whiting, wollastonite, feldspar, colemanite, or dolomite. It is the principle flux in medium and high fire glazes. In higher amounts it can give matte qualities through the formation of calcium silicate crystals.
- K2O - Potassium oxide is supplied by potash feldspar and cornwall stone. It is an important auxiliary flux in high temperature glazes. It has a high expansion.
- Na2O - Sodium oxide is supplied by feldspar, nepheline syenite and sodium frits. A slightly more powerful flux than potassium for high temperature glazes. It has a high expansion.
- MgO - Magnesium oxide is supplied by talc or dolomite. At lower temperatures, it is a matting agent and opacifier; at higher temperatures, it is an active alkaline flux.
- Fe2O3 , FeO, Fe3O4 - Ferrous-ferric oxide is supplied by iron oxide and stained clays. It is the most popular colorant. In a reducing atmosphere, it can act as a flux in both bodies and glazes at high temperatures.
- ZnO - Zinc oxide is available in a pure state. It is a low expansion secondary flux, in moderate to higher amounts it acts to produce mattes and crystalline surfaces.
- TiO2 - Titanium dioxide is available pure or in rutile. It is a complex material because of its opacifying, crystallizing, and multitude of color responses.
- ZrO2 - Zirconium oxide is available in a pure state and is supplied by zircon opacifiers. It is used to opacity glazes. Zirconium has a very low thermal expansion.
- BaO - Barium oxide is supplied by barium carbonate. It is a flux which encourages the growth of micro-crystals to produce attractive satin-matte surfaces. It also has unique color responses.
- Li2O - Lithium oxide is supplied by lithium carbonate or lithium feldspar (i.e. spodumene). It is a powerful auxiliary alkaline flux. Its expansion is lower than soda or potash.
- PbO - Lead oxide is supplied by lead frits. It reacts easily with silica to form low melting lead silicates of high gloss and deep character.
- SrO - Strontium oxide is supplied by strontium carbonate. It has matting and crystallizing properties similar to barium although it produces brighter and more fusible glazes with fewer surface defects.
Related Information
Ceramic Oxide Periodic Table
Pretty well all common traditional ceramic base glazes are made from less than a dozen elements (plus oxygen). Go to the full picture of this table and click or tap each of the oxides to learn more (on its page at digitalfire.com). When materials melt, they decompose, sourcing these elements in oxide form. The kiln builds the glaze from them, it does not care what material sources what oxide (assuming, of course, that all materials do melt or dissolve completely into the melt to release those oxides). Each of these oxides contributes specific properties to the glass. So, you can look at a formula and make a good prediction of the properties of the fired glaze. And know what specific oxide to increase or decrease to move a property in a given direction (e.g. melting behavior, hardness, durability, thermal expansion, color, gloss, crystallization). And know about how they interact (affecting each other). This is powerful. A lot of ceramic materials are available, hundreds - that is complicated when individual materials source multiple oxides. Viewing a glaze as a simple unity formula of ceramic oxides is just simpler.