Digitalfire will shut down on June 26. I no longer have the authority to grant exemption to a section in the Terms and Conditions of using material in the Insight-Live account from which I built the source material. While there are ways to comply with the take-down order, they are beyond my means because of how complex and large the site has become in the past 35+ years. It has been a wild ride for a shy prairie boy, thanks to everyone for your support.
All Articles
A ChatBot gives jaw-dropping glaze recipe advice - Jan 2025A Low Cost Tester of Glaze Melt FluidityA One-speed Lab or Studio Slurry MixerA Textbook Cone 6 Matte Glaze With ProblemsAdjusting Glaze Expansion by Calculation to Solve ShiveringAlberta Slip, 20 Years of Substitution for Albany SlipAn Overview of Ceramic StainsAre You in Control of Your Production Process?Are Your Glazes Food Safe or are They Leachable?Attack on Glass: Corrosion Attack MechanismsBall Milling Glazes, Bodies, EngobesBinders for Ceramic BodiesBringing Out the Big Guns in Craze Control: MgO (G1215U)Can We Help You Fix a Specific Problem?Ceramic Glazes TodayCeramic Material NomenclatureCeramic Tile Clay Body FormulationChanging Our View of GlazesChemistry vs. Matrix Blending to Create Glazes from Native MaterialsConcentrate on One Good GlazeCopper Red GlazesCrazing and Bacteria: Is There a Hazard?Crazing in Stoneware Glazes: Treating the Causes, Not the SymptomsCreating a Non-Glaze Ceramic Slip or EngobeCreating Your Own Budget GlazeCrystal Glazes: Understanding the Process and MaterialsDeflocculants: A Detailed OverviewDemonstrating Glaze Fit Issues to StudentsDiagnosing a Casting Problem at a Sanitaryware PlantDrying Ceramics Without CracksDuplicating Albany SlipDuplicating AP Green FireclayElectric Hobby Kilns: What You Need to KnowFighting the Glaze DragonFiring Clay Test BarsFiring: What Happens to Ceramic Ware in a Firing KilnFirst You See It Then You Don't: Raku Glaze StabilityFixing a glaze that does not stay in suspensionFormulating a body using clays native to your areaFormulating a Clear Glaze Compatible with Chrome-Tin StainsFormulating a PorcelainFormulating Ash and Native-Material GlazesG1214M Cone 5-7 20x5 glossy transparent glazeG1214W Cone 6 transparent glazeG1214Z Cone 6 matte glazeG1916M Cone 06-04 transparent glazeGetting the Glaze Color You Want: Working With StainsGlaze and Body Pigments and Stains in the Ceramic Tile IndustryGlaze Chemistry Basics - Formula, Analysis, Mole%, Unity Glaze chemistry using a frit of approximate analysisGlaze Recipes: Formulate and Make Your Own InsteadGlaze Types, Formulation and Application in the Tile IndustryHaving Your Glaze Tested for Toxic Metal ReleaseHigh Gloss GlazesHire Us for a 3D Printing ProjectHow a Material Chemical Analysis is DoneHow desktop INSIGHT Deals With Unity, LOI and Formula WeightHow to Find and Test Your Own Native ClaysI have always done it this way!Inkjet Decoration of Ceramic TilesIs Your Fired Ware Safe?Leaching Cone 6 Glaze Case StudyLimit Formulas and Target FormulasLow Budget Testing of Ceramic GlazesMake Your Own Ball Mill StandMaking Glaze Testing ConesMonoporosa or Single Fired Wall TilesOrganic Matter in Clays: Detailed OverviewOutdoor Weather Resistant CeramicsPainting Glazes Rather Than Dipping or SprayingParticle Size Distribution of Ceramic PowdersPorcelain Tile, Vitrified TileRationalizing Conflicting Opinions About PlasticityRavenscrag Slip is BornRecylcing Scrap ClayReducing the Firing Temperature of a Glaze From Cone 10 to 6Setting up a Clay Testing Program in Your Company or StudioSimple Physical Testing of ClaysSingle Fire GlazingSoluble Salts in Minerals: Detailed OverviewSome Keys to Dealing With Firing CracksStoneware Casting Body RecipesSubstituting Cornwall StoneSuper-Refined Terra SigillataThe Chemistry, Physics and Manufacturing of Glaze FritsThe Effect of Glaze Fit on Fired Ware StrengthThe Four Levels on Which to View Ceramic GlazesThe Majolica Earthenware ProcessThe Potter's PrayerThe Right Chemistry for a Cone 6 Magnesia MatteThe Trials of Being the Only Technical Person in the ClubThe Whining Stops Here: A Realistic Look at Clay BodiesThose Unlabelled Bags and BucketsTiles and Mosaics for PottersToxicity of Firebricks Used in OvensTrafficking in Glaze RecipesUnderstanding Ceramic MaterialsUnderstanding Ceramic OxidesUnderstanding Glaze Slurry PropertiesUnderstanding the Deflocculation Process in Slip CastingUnderstanding the Terra Cotta Slip Casting Recipes In North AmericaUnderstanding Thermal Expansion in Ceramic GlazesUnwanted Crystallization in a Cone 6 GlazeUsing Dextrin, Glycerine and CMC Gum togetherVolcanic AshWhat Determines a Glaze's Firing Temperature?What is a Mole, Checking Out the MoleWhat is the Glaze Dragon?Where do I start in understanding glazes?Why Textbook Glazes Are So DifficultWorking with children Low Budget Testing of Ceramic Glazes
Description
There is more to glazes than their visual character, they have other physical properties like hardness, thermal expansion, leachability, chemistry and they exhibit many defects. Here are some simple tests.
Article
What if you could greatly increase the quality of your fired ware by only small changes? Would you do it? Testing it thoroughly is a key ingredient. But mention the idea of testing a glaze and 99% of us think in terms of dipping a test tile and firing it to see how it looks. Many have learned that there is often little correlation between how a glaze looks on a little test tile compared with how it looks when used on ware, thus they tend to put little effort into testing. However if you already have a glaze in production, or have made an adjustment to an existing one, you are likely willing to expend much more effort to evaluate it fully.
Raw and fired glazes exhibit many properties that both production and end users are knowingly or unknowingly concerned with. These include slurry properties, dry hardness, behavior of the melt, freezing characteristics, hardness and scratch resistance of the fired glass, compatibility of host glaze and added colorants, leach resistance, glaze fit with the body, clarity of the fired glass, etc. Certain factors such susceptibility to material change and varying firing conditions are more difficult to measure.
Most people and companies do not have fancy glaze testing equipment to evaluate these properties. It is to these that this article is directed, there is much you can do to greatly increase your confidence in the true 'quality' of your product. Testing your glaze thoroughly is doubly important if you are using one or two base glazes because, in a sense, you have all your 'quality eggs in one basket'. We 'hoot' a lot about the advantages of focusing your efforts on one base glossy and matte recipe and altering these to make whatever you want. Thus the following tests all assume and depend on the fact that you are testing the transparent base without any colorants, opacifiers, or other additives. Remember that improving the base improves every recipe that is based on it.
Here are some tests you should consider:
- Slurry Properties
Mix a small pail of the glaze and bring it to the proper consistency (I am assuming you are glazing bisque ware). Most glazes work best when there is enough water to make them fluid and not so much that they do not gel. Typically you should be able to stir a glaze with a stick, pull the stick out, and the slurry should remain in motion only for 2-4 seconds. Measure its specific gravity and record this amount. If in future the glaze gels, settles, or runs excessively check its specific gravity. If it is correct then you need to investigate changes in your water supply or dry materials that could flocculate or deflocculate the slurry.
Let the container of glaze sit overnight and check it the next day for any tendency to settle or gel excessively. If it settles incorporate some bentonite in the recipe. If it gels to the point that remixing does not thin it out then replace materials known to be soluble (i.e. Gerstley Borate, Nepheline Syenite) or use distilled water.
- Application Properties
Dip your dry finger into the slurry and pull it out. Only one or two drips should fall and a good layer of glaze should hold itself in place. For glazes intended for application to bisque ware, dip a thick test tile (2 cm thick) all the way in for two seconds, pull it out and turn it over and watch for any tendency to run and drip. Note how quick it dries. When dry dip it again half way and hold it in for several seconds. Set it out to dry and note any tendency of the glaze cover to crack during drying (this is an indication of too much clay or too plastic clay in the recipe). When the specimen is completely dry note its tendency to 'powder off' in your hands. Will it accept overglaze painted decoration without turning to mud or will wax resist paint on and hang on well (if not the clay content is either too low or not plastic enough).
Dip a thin test tile also (5mm thick or less) and apply thick and thin layers as above (the tile should be thin enough so that the clay becomes waterlogged and the glaze thus dries slowly). Note any tendency of the glaze to bubble as it dries, this indicates that the specific gravity of the glaze may be too low.
- Crystallization, Clarity, Crawling
Fire the thick and thin test specimens made above. The thick one will cool slower, note any tendency for it to devitrify (develop crystals) compared to the thin one. Note any tendency toward crawling on the thickly glazed sections of the specimens, especially near edges. Note any tendency of the glaze to cloud with bubbles in the thicker areas.
- Stain Compatibility
Using a small brush paint stain ID numbers and color swatches on a flat tile of the target clay body. Glaze the whole tile over with a transparent version of the base glaze you are testing and fire. Note colors that are off and research the required chemistry to explain why.
- Leaching
Add a colorant like cobalt to a transparent version of the glaze being test, make and fire a bowl, fill it with vinegar and leave it in a warm place for twenty four hours. Note any fading of color, reformulate and test again till no leaching occurs.
- Hardness
Take a sharp concrete nail and attempt to scratch the glaze. Compare its performance against a benchmark glaze that has proven to be durable. Or use a hardened steel file to attempt to remove glaze on the lip or corner of a piece.
- Cutlery Marking
Using the edge of a stainless spoon or fork attempt to mark the surface of the glaze. If it marks attempt to rub or clean the mark off. If you cannot consider reformulating the glaze to develop a smoother surface or fewer crystals, flux it to melt more, or fire it higher.
- Crazing, Shivering
Cycle a thin glazed shard of your body-glaze combination between three-minute immersions in boiling water and ice water. Do it three times. Use a black marker to color an area of the surface. Clean the ink off using methyl hydrate. Note any craze lines highlighted by the ink. Note any areas near edges that may be flaking off (shivering). Reformulate the glaze to reduce its thermal expansion (increase it for shivering), fire, and test again.
- Glaze Over Solubles
Prepare a 12cm diameter disk 5mm thick from your clay and dry it under a fan with the center 6 cm covered. Any soluble salts in your clay body will be amplified on the outer 3cm ring. Break the disk in half, glaze half, and support and fire it resting on the flat. Note any reaction between the soluble salts in your clay and the glaze (i.e. blistering, orange peeling).
- Flow
Check the flow of the melt using a flow tester.
- Fired Volatility
Many glazes work well at one temperature but if fired slightly higher or lower they can have a much different surface. This type of behavior is normally only tolerated in very special purpose glazes. Thus you should prepare sample tiles for firing one cone higher and lower than you working temperature. This will help you spot possible trouble in future if kiln firings are not totally consistent.
- Microscope
Using a $20 30X Lightscope (available at hardware stores) look carefully at the glaze surface for any signs of poor melting (especially in matte glazes) or surface pits that could harbor bacteria. Identify any tiny specks as either impurities or the first stages of crystals. Break a shard and check for a good interface between glaze and clay. Examine any scratches you were able to make with the concrete nail.
- Make Functional Ware
Mix a couple of gallons of the base glaze and make a variety of functional ceramic shapes, glaze, and fire them. Note any problems like pinholing, crawling, bubbling, devitrification, and blistering.
Related Information
Feldspars, the primary high temperature flux, melt less than you think.

This picture has its own page with more detail, click here to see it.
Our melt fluidity tester is being used to compare cone 8 melt fluidities of Custer, G-200 and i-Minerals high soda and high potassium feldspars. Notice how little the pure materials are moving (bottom), even though they are fired to cone 11. In addition, the sodium feldspars move better than the potassium ones. But feldspars do their real fluxing work when they can interact with other materials. As a demonstration of that, note how well they flow with only 10% frit added (top), even though fired three cones lower.
Confirming slip viscosity using a paint-measuring device

This picture has its own page with more detail, click here to see it.
A Ford Cup is being using to measure the viscosity of a casting slip. These are available at paint supply stores. This is a #4 (4.25mm opening), it holds 100ml and drains water in 10 seconds. This casting slip has a specific gravity of 1.79. Having made it many times, our experience indicates 40-seconds as a drain target (after high energy mixing). In production situations, the seconds-value this test produces enables an audit-trail for quality control and problem solving. When first mixing a slurry, under-deflocculating and eye-balling the viscosity is typical, during that period the slurry gels while draining and Ford cup measurements are not valid. When the mixing process has been perfected and viscosity stabilized the Ford Cup becomes practical.
Don’t overthink this type of measurement or the type of cup or opening size (you can even make your own cup). You must still determine the optimal flow rate based on experience with your process. This technique is more about maintaining to ongoing adherence to a standard you define.
A batch of fired clay test bars in the Plainsman Clays lab

This picture has its own page with more detail, click here to see it.
A batch of fired test bars that have just been boiled and weighed, from these we get dry shrinkage, fired shrinkage and porosity. Each pile is a different mix, fired to various temperatures. Test runs are on the left, production runs on the right. Each bar is stamped with a code number and specimen number (the different specimens are the different temperatures). The measurements have all been entered into our group account at insight-live.com. Now I have to lay out and photograph each pile and upload the picture into the code-numbered record. Upon doing so I compare color and tests results to make decisions on what to do next (documenting these in insight-live).