Alternate Names: Stannic Oxide, Tin(IV) Oxide, Tin Dioxide, SnO2
Formula: SnO2
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| SnO2 | 100.00% | 1.00 | |
| Oxide Weight | 150.71 | ||
| Formula Weight | 150.71 | ||
Tin oxide is a white or off-white powder produced by oxidizing molten high-grade tin metal. It is typically quite pure, some manufacturers have grades up to 99.999% purity. Tin oxide powder is very fine-grained and it agglomerates, so glazes containing it need to be sieved to break down the small lumps (even a high-speed propeller mixer often won't do it).
Tin oxide has long been used to opacify glazes in oxidation (make transparents opaque) at all temperatures. Hand-decorated tin-glazed earthenware of the 1700s/1800s is the most famous use of tin in glazes (delftware-England, faience-France, maiolica-Italy). While many potters are keeping this tradition alive today, most now use zircon-based opacifiers instead. Thus any discussion about the use of tin oxide as an opacifier ends up comparing it with zircon products:
-Twice as much zircon is required to produce the same level of opacity.
-Like zircon, tin melts at very high temperatures and thus does not go into solution in typical glaze melts.
-Zircon will stiffen the glaze melt more than tin.
-Zircon will produces a harder glaze surface, but that surface can have cutlery marking issues.
-Zircon will reduce the thermal expansion of the glaze more than tin.
-The quality of the white color is different (tin tends to be more of a blue white, zircon a yellowish white).
-Tin is very expensive. That being said, it has double the potency and tin glazes can be applied thinner, these two factors can even out the cost.
-Zircon tends to have less of an effect on the development of metal oxide colors (e.g. tin reacts with chrome to make pink).
-Tin can often produce and maintain better gloss.
-While there are other products that produce varying degrees of opacity, none are as neutral and non-reactive as tin and zircon. Other opacifiers also tend to variegate the glaze.
-Tin does not normally opacify in reduction firings.
Tin is also a player in the development of ceramic colors, for example, chrome tin pinks and maroons. Tin with iron in oxidation makes a warmer shade of brown than zirconium does.
Tin oxide is also a variegator. For example, tin can react with titanium and rutile to completely transform the color and character of a glaze. Although tin is expensive, very little is required to produce stunning effects in many colored glazes.
Some claim that a little tin (not enough to opacify) will add extra smoothness and shine to many glazes.
Tin oxide is also used (in high percentages) to make semi-conduction glazes in porcelain insulators.

This picture has its own page with more detail, click here to see it.
Made in Italy by Oximet Srl.

This picture has its own page with more detail, click here to see it.
This is the G1214Z1 calcia matte base (as opposed to the magnesia matte G2934). The clay is Plainsman M390. 5% Zircopax was added on the left (normally 10% or more is needed to get full opacity, the partially opaque effect highlight contours well). 5% tin oxide was added to the one on the right (tin is a more effective, albeit expensive opacifier in oxidation). The PLC6DS firing schedule was used.

This picture has its own page with more detail, click here to see it.
This is a cone 04 glaze on a terra cotta body. Two 300-gram test batches were made. Both have 5% tin oxide added to a base transparent, G1916Q. The one on the left was high-speed propeller-mixed for 10 seconds. That was not enough, small agglomerates appear as tiny white specks floating in the glass. The one on the right was blender mixed for 60 seconds. Now the incredibly small tin particles have been dispersed and can do their job of opacifying the glaze. Would sieving the slurry have worked? No, the particle agglomerates can be far smaller than the openings in an 80-mesh sieve (individual particles could be 1000 times smaller!). The thorough dispersion of the expensive tin oxide particles has real benefit: It enables making an accurate assessment of whether the 5% addition is enough. In this case it isn't, more is needed.

This picture has its own page with more detail, click here to see it.
The body is Plainsman M390. The firing schedule is Plainsman PLC6DS.

This picture has its own page with more detail, click here to see it.
The body is Plainsman M390. The firing schedule is Plainsman PLC6DS. Of course, rutile could be used in place of titanium; it contains iron oxide that would enhance the development of blue. A small amount of cobalt can also be added to enhance the blue (the G2934 magnesia matte on the left, especially, will respond to that).

This picture has its own page with more detail, click here to see it.
The body is Plainsman M390. The firing schedule is Plainsman PLC6DS. The tin is on the right.

This picture has its own page with more detail, click here to see it.
The body is Plainsman M390. The firing schedule is Plainsman PLC6DS.

This picture has its own page with more detail, click here to see it.
On Plainsman H443 iron stoneware in reduction firing. Notice Tin does not work. Also notice that between 7.5 and 10% Zircopax provides as much opacity as does 15% (Zircon is very expensive).

This picture has its own page with more detail, click here to see it.
This melt fluidity tester compares two different tin oxides in a cone 6 transparent glaze (G2926B). Opacifiers affect not just opacity in glazes, but also liquid properties of the melt. The length, surface character, opacity and color of these flows provide an excellent indication of how similar the two materials are. This is the GLFL test.

This picture has its own page with more detail, click here to see it.
This is a 45:27:28 Gerstley Borate:Kaolin:Silica base on a dark firing clay body. But tin oxide will do that in almost any cone 6 clear glaze (use one that fits your clay body).

This picture has its own page with more detail, click here to see it.
These two are the same Alberta Slip glaze, GA6-C, except the one on the right has 4% tin added (to the base which is Alberta Slip 80, Frit 3134 20, Rutile 4).

This picture has its own page with more detail, click here to see it.
Same body, same glaze. Left is cone 10 oxidation, right is cone 10 reduction. What a difference! This is a Ravenscrag-Slip-based recipe on a high-fire iron stoneware. In reduction, the iron oxide in the body and glaze darkens (especially the body) and melts much more. The behavior of the tin oxide opacifier is also much different (having very little opacifying effect in reduction).

This picture has its own page with more detail, click here to see it.
Right: Ravenscrag GR6-A transparent base glaze. Left: It has been opacified (turned opaque) by adding 10% Zircopax. This opacification mechanism can be transplanted into almost any transparent glaze. It can also be employed in colored transparents, it will convert their coloration to a pastel shade, lightening it. Zircon works well in oxidation and reduction. Tin oxide is another opacifier, it is much more expensive and only works in oxidation firing.

This picture has its own page with more detail, click here to see it.
This is the G2571A base dolomite matte recipe. The specimen on the left adds 4% tin and 1% iron oxide. The one on the right has 4% tin oxide and 0.5% iron oxide.

This picture has its own page with more detail, click here to see it.
This is Alberta Slip (GA6C) on the left. Added frit is melting the Alberta Slip clay to it flows well at cone 6 and added rutile is creating the blue variegated effect (in the absence of expensive cobalt). However GA6D (right) is the same glaze with added Tin Oxide. The tin completely immobilizes the rutile blue effect, it brings out the color of the iron (from the rutile and the body).

This picture has its own page with more detail, click here to see it.
Both of these mugs were soaked 15 minutes at cone 6 (2200F), then cooled at 100F per hour to 2100F and soaked for 30 minutes and then cooled at 200F/hour to 1500F. This firing schedule was done to eliminate glaze defects like pinholes and blisters. Normally the GA6-A glaze crystallizes (devitrifies) heavily with this type of firing, but an addition of 1% tin oxide to the one on the left has prevented this behavior.

This picture has its own page with more detail, click here to see it.
The body is Plainsman M390. Firing is the cone 6 PLC6DS schedule. Each horizontal row is a commonly-used base glaze. The top one is a magnesia matte, the next one down is a calcia matte, row 3 is G2926B glossy and row 4 is Ravenscrag Slip+frit. The two mattes behave very differently from each other with the additions of opacifier. Thickly applying an opacified glaze will obviously affect visual character (column 4). Tin oxide fires whiter than zircon (e.g. Zircopax). If you like the G2934 recipe, consider the G2934Y variant for better melting.

This picture has its own page with more detail, click here to see it.
These samples illustrate 4, 5, 6 & 7% tin oxide added to a transparent. Tin is super expensive (Zircopax costs five times less at time of writing). But consider some advantages of tin. It creates a whiter glaze. A tin-opacified glaze may only need to be half as thick as a zircon-opacified one. Only half the percentage is required in recipes. Tin does not reduce the glaze's thermal expansion as much. On these samples, the higher percentages of tin seem to produce an even better glossy surface. Tin is less likely to cause crawling, a classic issue with high-zircon glazes (it impedes melt fluidity, that is what holds super thickly applied majolica glazes on the ware). Tin is the opposite; even though this recipe is high in strontium, and thus has a high surface tension, there is no indication of crawling with the tin addition. A final issue is cutlery marking, a common problem with zircon-opacified glazes. But not with tin oxide.

This picture has its own page with more detail, click here to see it.
The glaze is G2926B, our standard base transparent. The Zircopax (zircon) is Ultrox Z+. We made a range of test pieces and found these two versions remarkably similar. The tin oxide version is a little bluer for some pieces, on others, it was difficult to distinguish them. We even tried the two glazes on a jet-black engobe, the opacification was similar there also. The cost? At our current retail pricing, 1000 g of glaze powder requires $5.70 worth of tin oxide vs. $1.72 of zircon (to make a gallon would be about twice those). But a critical issue is crawling, high zircon whites are notorious for this. We thus now use mix of tin and zircon (3% and 5%) for tableware. The sanitaryware industry would not likely be able to justify this expense so they are motivated to investigate other options (e.g. adjust the melt surface tension by glaze chemistry or compensate by better laydown and dry adhesion).
| URLs |
http://mineral.galleries.com/minerals/oxides/cassiter/cassiter.htm
The Mineral Cassiterite |
| URLs |
http://en.wikipedia.org/wiki/Tin_dioxide
Tin Oxide at Wikipedia |
| Materials |
Zirconium Dioxide
|
| Materials |
Zircopax
Zirconium silicate, its principle use in ceramics is as an opacifier in glazes. It is an expensive material, but less so than tin oxide. |
| Materials |
Zircopax Plus
|
| Materials |
Zircon
Zircon (zirconium silicate) is a hard, dense, refractory ceramic material used to opacify pottery glazes and in refractory products such as kiln washes, crucibl |
| Typecodes |
Generic Material
Generic materials are those with no brand name. Normally they are theoretical, the chemistry portrays what a specimen would be if it had no contamination. Generic materials are helpful in educational situations where students need to study material theory (later they graduate to dealing with real world materials). They are also helpful where the chemistry of an actual material is not known. Often the accuracy of calculations is sufficient using generic materials. |
| Typecodes |
Opacifier
Opacifiers are powders that turn transparent glazes opaque by various chemical and physical mechanisms (and combinations of mechanisms). |
| Glossary |
Opacifier
Glaze opacity refers to the degree to which it is opaque. Opacifiers are powders added to transparent ceramic glazes to make them opaque. |
| Glossary |
Metal Oxides
Metal oxide powders are used in ceramics to produce color. But a life time is not enough to study the complexities of their use and potential in glazes, engobes, bodies and enamels. |
| Glossary |
Variegation
Ceramic glaze variegation refers to its visual character. This is an overview of the various mechanisms to make glazes dance with color, crystals, highlights, speckles, rivulets, etc. |
| Oxides | SnO2 - Tin Oxide, Stannic Oxide |
| Minerals |
Cassiterite
Tin oxide mineral. |
| Glaze Opacifier | As little as 4-7% can produce brilliant white, although it is more typical to use 8-10% for full opacity. However, be aware that even tiny amounts of chrome in the kiln will volatilize and combine with the tin to produce pink shades. |
|---|---|
| Glaze Variegation | Tin reacts with iron in fluid glazes to produce variegated surfaces. A good example is the Albany Slip 85, Tin 4, Lithium 11 glaze for cone 6. |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk