3D Print a Test of the Beer Bottle Neck
3D Printing a Clay Cookie Cutter-Stamper
A 3-minute Mug with Plainsman Polar Ice
A Broken Glaze Meets Insight-Live and a Magic Material
Accessing Recipes from "Mid-Fire Glazes" book in Insight-Live
Adjusting the Thixotropy of an Engobe for Pottery
Analysing a Crazing, Cutlery-marking Glaze Using Insight-Live
Compare the Chemistry of Recipes Using Insight-Live
Connecting an External Image to Insight-Live Pictures
Converting G1214M Cone 6 transparent glaze to G1214Z matte
Create a Synthetic Feldspar in Insight-Live
Creating a Cone 6 Oil-Spot Overglaze Effect
Design a Triangular Pottery Plate Block Mold in Fusion 360
Designing a Jigger Mold for a Bowl Using Fusion 360 CAD
Downloading and 3D-Printing a 3MF file
Draw a propeller in Fusion 360 for use on an overhead propeller mixer
Drawing a Mug Handle Mold in Fusion 360
Drawing a Mug Mold Using OnShape CAD
Enter a Recipe Into Insight-live
Entering TestData Into Insight-Live
Fine tune the thixotropy of a glaze or engobe slurry
Getting frustrated Gerstley Borate turning glazes to jelly
How I Developed the G2926B Cone 6 Transparent Base Glaze
How I Formulated G2934 Cone 6 Silky MgO Matte Glaze Using Insight-Live
How to Apply a White Slip to Terra Cotta Ware
How to Paste a Recipe Into Insight-live
Importing Data into Insight-live
Importing Desktop Insight Recipes to Insight-live
Importing Generic CSV Recipe Data into Insight-Live
Insight-Live Meets a Silica Deprived Glaze Recipe
Insight-Live Quick Tour
Liner Glazing a Stoneware Mug
Make a precision plaster mold for slip casting using Fusion 360 and 3D Printing
Making ceramic glaze flow test balls
Making test bars for the SHAB, LDW and DFAC tests
Manually program your kiln or suffer glaze defects!
Mica and Feldspar Mine of MGK Minerals
Predicting Glaze Durability by Chemistry in Insight-Live
Preparing Pictures for Insight-live
Replace Lithium Carbonate With Lithium Frit Using Insight-Live
Replacing 10% Gerstley Borate in a clear glaze
Same Beer Bottle Mold Using Fusion 360 and OnShape CAD
Signing Up at Insight-live.com
Signing-In at Insight-live.com
Slip cast a stoneware beer bottle
Substitute Ferro Frit 3134 For Another Frit
Substituting Custer Feldspar in a Cone 10R glaze recipe
Thixotropy and How to Gel a Ceramic Glaze
Use Insight-live to substitute materials in a recipe
Watch Thixotropy Happen With a 20kg Batch of Dipping Glaze

Substitute Ferro Frit 3134 For Another Frit

I use my Insight-live account to do the glaze chemistry to replace Ferro frit 3134 with combinations of three other common Ferro frits. We will see the challenges of doing this in three different types of recipes.

You can also watch this at Screencast-o-matic.com

Transcript/Notes

First look at the glaze flow test that compares 3124 with 3134: They fire much different, 3124 does not melt nearly as well.

Recipe 1:
In my Insight-live account I'll open the first one, it has 20% frit 3134.
Duplicate it, edit the 3134 line to 3124, click Done and turn on the formula.

more.. The Al2O3 and SiO2 are up, the B2O3 is down.
In calculation mode increase the frit from 20 to 35 to match the B2O3.
But now the Al2O3 and SiO2 are high. Drop the kaolin and silica to re-match them.
That was easy. We used more 3124 and dropped kaolin and silica.

Recipe 2:
It is more tricky because the B2O3 is double, there is more frit, there is only 10% kaolin. I will have to cut the feldspar to reduce the Al2O3.
Duplicate the recipe, change the frit, click Done and turn on the formula.
In calculation mode, reduce the feldspar until the Al2O3 matches - removing all fo the feldspar does not reduce the Al2O3 enough! And the B2O3 is high and alot of KNaO has been lost.
We need a frit that is high in sodium, low in boron and alumina: Frit 3110
Add 10 parts 3110 and reduce the other frit by the same. Bump up the 3110 to re-match the KNaO. We lost B2O3 in doing that.
We need a more concentrated source of boron: Frit 3195. Add 10 to the recipe and reduce 3124 by 10. Remove the feldspar and increment the 3195 by 5 and decrement the 3124 by 5 until the boron matches.
Nudge the kaolin down until the Al2O3 matches.
Retotal the recipe to 100.
The cost is up. We ended up removing the feldspar and replacing frit 3134 with three other frits.

Recipe 3:
The frit percentage is high and there is plenty of clay and silica.
Duplicate and replace the frit as in the others.
The boron is down and the Al2O3 and SiO2 have skyrocketed.
Reduce the kaolin and silica to re-match the Al2O3 and SiO2.
Boron was lost, we need help from a more concentrated boron frit: Add 15 frit 3195 and reduce the 3124 by the same.
In calculation mode reduce 3195 and increase 3124 until B2O3 matches.
Fine tune the Al2O3 and SiO2 by adjusting kaolin and silica.
Retotal the recipe and assess what we did.
The EPK was cut in half (but still enough to float the slurry) and silica is down also.
A mix of 3124 and 3195 supplied the boron and other fluxes.

Using this chemistry approach brings a high degree of confidence that the adjusted recipes will fire the same as the originals.



Links

Media Create a Synthetic Feldspar in Insight-Live
A step-by-step of how to duplicate the chemistry of Minspar by mixing other materials. You will learn the calculate process, the type of testing to do and how to keep track of the results with notes, pictures and links.

Substitute Ferro Frit 3134, using glaze chemistry, in three glaze types


Insight-live screen shot, substituting frit 3134

This picture has its own page with more detail, click here to see it.

Can't get frit 3134 for glaze recipes? Can you replace it with frit 3124? No, 3124 has five times the amount of Al2O3 (the second most important oxide in glazes) and half the amount of B2O3 (the main melter). This ten-minute video presents a glaze chemistry approach that is easier to do than you probably think. It deals with three different glaze recipe types lacking sufficient clay to suspend the slurry. Learn to source the needed oxides from two other Ferro frits, 3110 (or Fusion F-75) and 3195 (Fusion F-2), and end up with at least 15% kaolin in each. A unique approach is required in each situation. Two of the calculations produce improved slurry properties and one yields a recipe of significantly lower cost. If you have a recipe that needs this and need help please contact us.

Is Ferro Frit 3124 a viable substitute for Frit 3134?


Three melt from tests comparing these frits

This picture has its own page with more detail, click here to see it.

This is a GLFL test comparing the melt flow of the three materials at 1800F. Frit 3124 is barely out of the starting gate and the other two have crossed the finish line! With frits chemistry is a big deal, they are all about supplying oxides to the melt. Frit 3134 is low-alumina/high-boron, 3124 is medium-alumina/low-boron and 3195 is medium-alumina/high-boron. Boron is the melter. Alumina thickens the melt and hardens the glass. Just from this it appears that Frit 3195 is a better starting point for calculations to replace frit 3134.

Clay is dirt. Glaze is powdered rock and glass.

Why do they cost so much? DIY is the answer.


Shipping containers piled high

This picture has its own page with more detail, click here to see it.

Historically, pottery has been a shining star of resilience and independence because the materials were in the ground nearby. So why are they coming thousands of miles in shipping containers? Because you can't just head out to the nearest hill with your wheelbarrow. But you are not helpless either.

Rather than viewing these containers as full of specific brand-name clays, minerals and man-made powders, it is better to view them as full of materials that supply the physical properties and chemistries needed to make bodies, glazes, engobes, slips, etc. By characterizing your glazes and bodies, using an effective record-keeping system, you can not only adjust recipes to adapt to changing supplies, but even improve them in the process (adjusting glaze thermal expansion, temperature, surface, color, etc). Or, use materials native to your area. It is not rocket science; it is just work and gradual learning accompanied by organized record-keeping, good labelling and interpretation skills.

Click here for case-studies of Insight-Live fixing problems


Insight-live help button

This picture has its own page with more detail, click here to see it.

You will see examples of replacing unavailable materials (especially frits), fixing various issues (e.g. running, crazing, settling), making them melt more, adjusting matteness, etc. Insight-Live has an extensive help system (the round blue icon on the left) that also deals with fixing real-world problems and understanding glazes and clay bodies.

This pottery glaze is peeling when multi-layered:

The recipe reveals why.


Pottery glaze peeling

This picture has its own page with more detail, click here to see it.

Dipping glazes can, in very controlled circumstances, be multi-layered. If you have done it for some time, with success, you may have been just lucky. These pieces demonstrate one of many factors that can produce failure: The top glaze contains 7% bentonite and 5% zinc oxide - that is 12% hyper-fine particles, perfect to create the drying shrinkage to make this happen. The recipe author must have reasoned that it could "pinch hit" for the inadequate clay content. But 7% bentonite in any glaze is highly unusual. And, it is actually not even necessary here. Why? The high percentage of Ferro Frit 3124 is sourcing needless Al2O3 (alumina), that should be coming from kaolin or ball clay instead. Frit 3134 is the perfect stand-in, it contains almost no Al2O3, but otherwise is quite similar. The equivalent recipe we calculated on the right has the same chemistry, but does pass a sanity check. It is not guaranteed to work, but has a better chance than this one. For even more assurance of success, it should be mixed as a base-coat dipping glaze.


PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy