Lithium Carbonate

Alternate Names: Lith Carb, Li2CO3

Formula: Li2CO3

Oxide Analysis Formula Tolerance
Li2O 40.74% 1.00
CO2 59.26%n/a
Oxide Weight 29.80
Formula Weight 73.15

Notes

Lithium Carbonate is the best source of lithium oxide for glazes. It is slightly soluble and a powerful melter. However, its most important characteristic at this time is price, it is not sold by the gram! In early 2024 this material was costing us $7 for the 22 grams needed to make one jar of brushing glaze! Most recipes call for 5% or less, so the cost is still tolerable for hobbyists. But some reactive glazes contain much more, they are being discontinued by some manufacturers. In an unexpected turn, lithium prices suddenly fell by more than 60% because of a downturn in electric car production in China - however prices from ceramic suppliers won't drop until they sell current supplies and reorder (however prices are expected to rebound in future).

There are certain basic properties of lithium which are of interest in ceramics. Since lithium has a very small ionic radius in comparison to the other alkali metals, it has a higher field strength. Low expansion coefficients are generally imparted to ceramic compositions containing lithia (beneficial to glazes that tend to craze but harmful to ones already tending to shiver). Lithium carbonate is a very strong flux (also true of lithium fluoride). Because it is such an active melter lithium is valuable in the production of reactive glazes. In contrast, other lithium compounds may be quite refractory: lithium zirconate and lithium aluminum spinel are examples.

There is comparatively little published information on the use of lithia compounds in ceramics. Laboratory investigations indicate that small additions of lithium will react with quartz during firing and eliminate the alpha-beta quartz transition in the cooling cycle. Lithia imparts low thermal expansion coefficients to glasses and also promotes devitrification in glass systems. Smaller amounts act to smooth the glass surface.

Lithium exhibits many properties that are similar to the more common alkali metals sodium and potassium. In many respects it also shows similarities to the elements of the alkaline earth group, especially magnesium.

In addition to being soluble, lithium carbonate produces gases as it decomposes and these can cause pinholes or blisters in glazes. There are insoluble lithium frits available (e.g. Fusion F-493 has 11%) and incorporating one of them to source the Li2O instead is a classic application of glaze chemistry calculations (however for glazes with very high amounts of lithium, like 10%+, it will be difficult to source the Li2O using a frit because significant amounts will be required and this will likely oversupply the other oxides the frit brings). The resultant glaze will be more fusible and will have better clarity and fewer defects.

Lithium carbonate is the best source of Li2O for frits (but the most expensive one). Lithium sources are becoming so expensive that companies and discontinuing products using them. Potters can often justify using lithium if they make smaller quantities of glaze, especially brushing glaze, and use them up to make ware that will be sold.

Lithium carbonate powders can be very fine and somewhat grainy. The finer particled powders can deflocculate a glaze slurry, reducing the amount of water required (but also changing other rheological properties).

If you need to substitute this material in glazes and need help, just purchase a group account at Insight-live.com and we can work together to get it done (sourcing the Li2O from a frit or spodumene). We will make a step-by-step video of the initial calculation and then work together in your account to track trials, adjustments and retrials. You will end up with a glaze having better slurry properties, fewer bubbles and better fit.

Related Information

Original container of Albemarle Lithium Carbonate


This picture has its own page with more detail, click here to see it.

Original container of Rockwood Lithium Carbonate


This picture has its own page with more detail, click here to see it.

Frits instead of raw zinc, lithium, barium, strontium


zinc, lithium, barium, strontium oxide powders

This picture has its own page with more detail, click here to see it.

Raw material sources of zinc, lithium, barium, strontium have issues (e.g. precipitates in glaze slurries, toxicity, high drying shrinkage and carbon burnoff that affect laydown and fired surface defects like pinholes, blisters, orange peeling, crystallization). Yet the oxides that these materials supply to the glaze melt - ZnO, Li2O, BaO and SrO, can be sourced from frits which melt much better and remove most of the problems. Consider examples made by Fusion:
-Frit F-493 has 11% Li2O
-F-403 has 35% BaO
-F-581 has 39% SrO
-FZ-16 has 15% ZnO
These frits source other oxides but such are common in most glazes and glaze calculation can be used to retain the overall chemistry. Although these are expensive, the benefits are game changers. But there is a problem: Potters can't get these. Therefore they have difficulty creating the dazzling visual effects of many commercial glazes.

Li2O from Spodumene instead of Lithium Carbonate:

Good chemistry and economy, but bad physics


Two very melt fluid glazes

This picture has its own page with more detail, click here to see it.

Lithium carbonate is now ultra-expensive. Yet the reactive glaze on the left needs it. Spodumene has a high enough Li2O concentration to be a possible source here. It also has a complex chemistry, but the other oxides it contains are those common to glazes anyway. I did recipe rescue calculations and got a pretty good match in the formulas (lower section in the green boxes). Then I made 10-gram balls and did a GLFL test at 2200F.

Not surprisingly, this recipe is very runny; that's why the tiny yellow crystals grow during cooling. The new version fires very similarly, perhaps better. My calculated cost to mix these in 2022 was $17.84/kg vs. $10.40/kg. In 2026, the difference is even greater! But there is a practical cost: Poor slurry properties. The spodumene sources so much Al2O3 that 70% Alberta Slip had to be dropped to accommodate it! How does one use this type of glaze without ruining kiln shelves? Using a catcher glaze is one answer.

Crystals found growing in a glaze containing lithium carbonate


This picture has its own page with more detail, click here to see it.

Crystals found growing in a glaze containing 7% lithium carbonate, 7% titanium dioxide and 6% cadycal. Also had wollastonite, silica, koalin and nepheline syenite. Courtesy of Mark Rossier Pottery.

Lithium carbonate precipitation in one gallon of glaze


This picture has its own page with more detail, click here to see it.

This is one of the issues with using the material. These have to be screened out from time to time, if not they produce defects in fired ware. Better to employ a lithium frit to source Li2O.

Alberta Slip used in the common lithium-tin cone 6 glaze


This picture has its own page with more detail, click here to see it.

This is 85% Alberta Slip, 11% lithium and 4% tin fired at cone 6 in oxidation. Like the original Albany version, it has a very low thermal expansion (because of the high lithium content) and likes to shiver on many clay bodies.

Add 6% lithium carbonate to an Alberta Slip glaze:

And this happens!


Alberta slip + lithium carbonate glaze

This picture has its own page with more detail, click here to see it.

Left is G3933A, it is an 80:20 mix of G2934 matte and G2926B glossy cone 6 base recipes (plus a mix of iron oxide, tin oxide and rutile). The body is Plainsman Coffee Clay. Because of repeated issues with crawling, a project was started to create the same effect using Alberta Slip to supply as much of the chemistry as possible. Along that road, the opportunity arose to add lithium (to duplicate Amaco PC-32, a classic Albany/Lithium recipe). The glaze on the mug on the right is G3933G1, it adds 6% lithium carbonate. Lithium is a super powerful melter, turning this into a very reactive glaze! However, there is a down side: To make a 500ml jar of DIY brushing glaze, in 2023, required about $7 worth of lithium carbonate.

Testing a new brand of lithium carbonate


Testing lithium carboante in a glaze

This picture has its own page with more detail, click here to see it.

Lithium carbonate had reached stratospheric prices and we were searching for a different supplier. We had to be sure the material from a new manufacturer was the same. How? We found a wonky glaze having 6% of it (lithium is a very powerful flux so small percentages are normal). By 'wonky' I mean one that gives little priority to function - it runs, crystallizes and crazes like mad and fires very differently depending on temperature, clay and firing schedule. We glazed a variety of pieces using this recipe and found it to work equally crazily on them all! These two, the original lithium on the right and the new one on the left, looked the most interesting, likely because of being on a dark clay body (Plainsman M390). Obviously, this type of recipe is very sensitive to thickness, we attributed the difference to that. Good news in 2024: Prices have dropped more than 60%.

Lithium carbonate and Gerstley Borate in glazes:

What is the best way forward?


Four common lithium carbonate glazes

This picture has its own page with more detail, click here to see it.

Lithium is getting really expensive. These are four recipes submitted by a customer who wonders if there is a substitute. The answer is not simple; each glaze is a unique situation. Fortunately, lithium carbonate is almost always a minor addition (in the first two recipes it is 1% and 3%). Lithium is a powerful low-expansion flux; in some cases, a low-melting, low-expansion frit could perform the same function (e.g. Ferro 3249). Even for the 6.5%, as in the third one, this could still work. But in these cases, wouldn't it be better to continue using lithium? Even for the last one that has 9%? It's only expensive if you make glazes and don't use them. Perhaps a solution is to make them as brushing glazes; a 1-pint jar only needs about 350g of powder (that is only about 30g for recipe 4).

This situation can also be considered an opportunity to rationalize the recipes you use. Let's pretend that each of these might be used on functional ware and should measure up to common-sense recipe limits. The Gerstley Borate in three of these is also a red flag; it won't be available shortly (calculating how to source B2O3 from frits is better anyway). During that process, you might find that lithium is not even needed. Another issue is thermal expansion. Notice that one of these calculates to 8.5 and another to 9.6! Those are virtually certain to craze. Why not lower that number while removing the Gerstley Borate? Notice that two of these have clay percentages over 70% (Alberta Slip and Gerstley Borate), these are virtually certain to crack on drying (and crawl on firing), that can also be fixed. The percentage of titanium, Zircopax and rutile in the fourth one are highly likely to make it crystallize heavily on cooling produce problems with cutlery marking and staining.

Lithium and the dramatic surface of AMACO PC-32 Albany Slip Brown


Lithium albany brown glaze

This picture has its own page with more detail, click here to see it.

Left is G3933A; right is AMACO PC-32 Albany Slip Brown. PC-32 shows much greater movement and a stronger contrast between creamy areas and rich brown. AMACO identifies lithium carbonate in this product, and our own tests show that adding lithium carbonate to a related glaze can greatly increase melt fluidity and transform its appearance. That supports lithium’s importance here, although it does not reveal AMACO’s base recipe or lithium percentage.

Where PC-32 collects more thickly, it develops a lighter, more opaque appearance; over raised contours, it thins and breaks brown. Crystallization may contribute to the cream-colored areas, but opacity as a product of phase separation is another possible mechanism. This raises an interesting development challenge: Can a lithium-free formulation reproduce both the flowing melt and the distinctive cream–brown separation? With the cost of lithium materials it is easy to imagine development work is being done.

LOI-gassing and Spodumene produce this:

Melt fluidity with blisters that variegate, then heal


This picture has its own page with more detail, click here to see it.

This pitcher was made by Elora Pottery. Like everyone using glazes that require lithium (from Spodumene or Lithium Carbonate), they are facing the unbelievable price increases these materials are seeing. Staci actually calculated the weight applied to each piece, determining the $$ dip cost! Notice her material costs on the photo. During efforts to reduce the spodumene content, I noticed the expensive carbonate colorants and asked if these were causing blisters in the glaze (because of gassing associated with their LOI). When I saw this picture, it became clear that they are. But in a good way. Part of the variegation we are seeing is doubtless the mechanical disturbance they cause in the fluid-melt phase-separated glass. But the melt fluidity of the glaze appears to be sufficient to heal them and smooth out the glass during cooling.

What did we do about the spodumene? We calculated to use lithium carbonate to supply the Li2O instead - it took one fifth as much material. Still super expensive, but easier to use and more consistent.

Links

Materials Lithium Carbonate (Foote)
Materials Spodumene
Spodumene is a lithium sourcing feldspar, an alternative to lithium carbonate to supply Li2O to ceramic glazes. Contains up to about 8% Li2O.
Materials Fusion Frit F-493
This frit is very valuable for one simple reason: It is a higher-quality source of Li2O for glazes than raw lithium carbonate. It contains 11% Li2O.
Hazards Lithium Carbonate Toxicity
Hazards Lithium Toxicology
Typecodes Generic Material
Generic materials are those with no brand name. Normally they are theoretical, the chemistry portrays what a specimen would be if it had no contamination. Generic materials are helpful in educational situations where students need to study material theory (later they graduate to dealing with real world materials). They are also helpful where the chemistry of an actual material is not known. Often the accuracy of calculations is sufficient using generic materials.
Typecodes Flux Source
Materials that source Na2O, K2O, Li2O, CaO, MgO and other fluxes but are not feldspars or frits. Remember that materials can be flux sources but also perform many other roles. For example, talc is a flux in high temperature glazes, but a matting agent in low temperatures ones. It can also be a flux, a filler and an expansion increaser in bodies.
URLs http://en.wikipedia.org/wiki/Lithium_carbonate
Lithium Carbonate at wikipedia.com
Oxides Li2O - Lithium Oxide, Lithia
Media Replace Lithium Carbonate With Lithium Frit Using Insight-Live
Raw lithium carbonate can often be replaced with a lithium-containing frit if you can do the chemistry. And you can at insight-live.com.

Data

Solubility 1.3 g/100ml at 20 deg C

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy