Oct 22, 2026: We are working on protecting our servers against the PHP2Shell vulnerability just discovered. The CDN download server is back online. The digitalfire and insight-live servers were patched on Oct 21.
Michael Banks and Stuart Altmann talk about chemical analyses methods and their advantages and disadvantages. Also information on testing labs you can use.
Conveniences today tend to isolate us from the materials we use. By the same token, the convenience of computers and calculation software isolate us from the hard work done to provide us with the material formula numbers to work with. Most people are not aware of how a lab analyzes a material to determine its chemistry. Following are comments from two respected contributors to the Clayart discussion group on this subject.
From: Michael Banks
Here we use X-ray fluorescence spectrometry (XRF) and atomic absorption spectroscopy (AAS) routinely on raw material analyses. AAS is perfectly quantitative in the right hands! :) These methods report elemental compositions. Molar composition of the respective oxides can be spat out by the computer programs controlling both analytical methods.

Sample chart from XRF machine
The most common chemical analytical technique used is X-ray fluorescence spectrometry (XRF) which can determine the proportions and identity of the major oxides of materials of widely differing composition such as silicates, carbonates, sulphates and phosphates from below 0.01% to 100%. The analysis is rapid and non- destructive, but is generally impractical for determining elements lighter than fluorine. Samples containing light elements such as lithium and boron for example, are often analyzed by atomic absorption spectroscopy (AAS) or colorimetric methods.
Major oxide analysis by XRF can be carried out on as little as 0.5 g of material. The sample material can be analyzed as a pressed powder of fused into a glass disk using a suitable flux, such as lithium tetraborate. Using fused samples allows an evenly dispersed solid solution, which enables a wide range of matrix compositions to be accurately, determined through the normalization of both particle size and inter-element (matrix) effects.
XRF works by beaming x-rays onto the sample, which excites some of the electrons orbiting the atomic nuclei (inside the atoms of the elements present), to jump to higher energy orbitals. The empty space in the respective orbital shell is replaced by another electron dropping down from a higher energy level. The electron emits an x-ray photon in order to drop to the lower energy level. This process of atoms emitting secondary x-rays in response to excitation by a primary x-ray source is called x-ray fluorescence. The secondary x-ray photons are emitted by the atoms of the elements in the sample in characteristic discrete frequency peaks, their fingerprint line spectra.

An XRF machine in use
Sample holders are arrayed in the left foreground
The elements in the sample can therefore be identified by their spectral wavelengths for qualitative analysis and the intensity of the emitted spectral lines enables quantitative analysis. This is accomplished by directing the secondary (fluorescence) radiation from the sample into a narrow beam by slit collimator and onto a crystal plate. The crystal is commonly lithium fluoride. The various wavelengths in the beam are diffracted by the crystal lattice atoms in the plate off at various angles proportional to their frequency (analogous to white light passing through a prism). A radiation detector is rotated by degrees around an accurate track (goniometer) and the individual frequencies and their intensities thus measured. The on-board computer then reduces this data to elemental or oxide concentration figures.
For this method, the pulverized sample is usually digested (dissolved into solution) by mixtures of strong acids, normally perchloric and hydrofluoric acid. AAS works by beaming light of a set frequency through a gas flame (acetylene-oxygen, or acetylene-nitrous oxide) into which an aqueous solution of the sample has been vaporized. In this case (similarly to XRF), the orbital electrons in the flame plasma, absorb certain quanta of light from the beam in order to jump up to higher energy levels. But in the reverse to XRF, a detector opposite the light source measures the intensity of the loss of a particular frequency and the elemental (or oxide composition) computed in relation to a set of known aqueous standards run through the AAS alternately
with samples.
Elements present in the atmosphere of the sun and stars also produce absorption spectra. Numerous dark bands in the spectrum of light emitted by these objects are characteristic of the elements present. The dark bands are specific frequency photons that have been absorbed by the elements in the suns (or stars) atmosphere. Spectral analysis of sunlight is virtually long-distance AAS.
Only a few elements are not easily determined by XRF or AAS. Probably the only one of consequence commonly present in ceramic materials is boron. This can be determined by colorimetry. This entails preparing an aqueous solution of the sample, adding a reagent which produces a strong colour in the presence of boron ions and reading the intensity of this colour in relation to standards of known boron concentration. The colour intensity comparisons are normally read by machine but can also be done by eye (as in the old days). Hopefully by someone not colour- blind!
Those few elements or materials not analyzed by these methods, can be determined by other more specialized techniques such as inductively coupled plasma spectroscopy (ICP) - similar to high temperature AAS, neutron activation analysis (NAA), or wet chemical analysis other than colorimetry. Individual microscopic minerals can be analyzed, in-situ in a rock, by electron microprobe, or x-ray microprobe, which is virtually micro-XRF.
From: Stuart Altmann <salt@Princeton.EDU>
The chemical analysis is done in terms of mass (so-called "weight," though not really that). But thanks to Avogadro's number, we can readily convert from mass to the number of atoms or molecules. The number of molecules in one gram-mole of a substance, defined as the molecular weight in grams, is 6.022 times 10 to the 23rd power--which is Avogadro's number. For example, the molecular weight of oxygen is 32, so one gram-mole of oxygen has a mass of 32 g and contains 6.022 x 10^23 molecules. Isn't that conversion amazing?
Many techniques are used for analysis of chemical elements, depending on the level of accuracy required, the equipment on hand, and so forth. For a good description of available techniques, see the Encyclopedia Brittanica's Macropedia, under Analysis and Measurement. An ordinary, relatively inexpensive analysis provides values good to two (or three) significant figures, and that's probably all the accuracy you can expect --or need-- for most pottery work.
The most accurate apparatus now being used for routine chemical analysis is the high-resolution mass spectroscope, which can resolve a difference as small as one part in 10,000,000. With that kind of precision, you can tell the masses not just of chemical elements but of the various isotopes of an element, e.g. carbon-12 vs. carbon-14, or hydrogen vs. deuterium vs. tritium.
A unity formula does not indicate the number of molecules or parts of molecules. It indicates the relative amounts (proportions) of the listed oxides. This common confusion would be avoided if unity formulas were expressed as percentages instead of proportions--but that would probably lead to a different confusion, of thinking that these are the percentages of oxides in your recipe.
Here is a table showing what the lab provides. A number of pottery supply catalogs include them, and many of the companies that produce them post them on their web pages. Here, for example, is Feldspar Corporation's posted analysis of their G200 feldspar. Note that the analysis is given in terms of oxides of the various elements; that is the form commonly used in glaze and clay calculations.
Typical Analysis
SiO2 66.3% Al2O3 18.5% Fe2O3 0.082% CaO 0.81% MgO TRACE Na2O 3.04% K2O 10.75% LOI 0.16%
I guess the only thing here that requires explanation is LOI, loss on ignition. This includes volatile material, such as the oxides of C, S, H, and N, some of which is from organic material. An analysis of sulfur content, which is important (negatively) to the potter, would usually have to be requested separately.
Depending on the equipment used in the chem lab and what is requested, the analysis may be given for the elements themselves, not their oxides. For example, analysis of water from a swamp in Amboseli National Park, Kenya, gave me the following:
Element Result (mcg/ml) Detection Limit Na 12400 mcg/ml 10 Fe 18.7 0.03 Mg 73.1 73.8 (etc., for 32 elements)
The more heterogeneous the material, the larger the sample size needed to achieve any given degree of accuracy in estimating mean composition. Getting representative samples is fraught with potential biases; much attention has been directed to methods for minimizing them. Do mining companies make use of modern sampling methods? Ah, thereby hangs a tale!
For a lab near you search for "chemical analysis service for ceramic oxides" on a search engine or visit the Thomas Register at http://www.thomasregister.com and look for labs that use the type of equipment listed here. Digitalfire also maintains a list of labs at https://digitalfire.com/services/database.php?list=labs
| URLs |
https://digitalfire.com/services/database.php?list=labs
Laboratories who can can do a chemical analysis on a material |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk