3D Print a Test of the Beer Bottle Neck
3D Printing a Clay Cookie Cutter-Stamper
A 3-minute Mug with Plainsman Polar Ice
A Broken Glaze Meets Insight-Live and a Magic Material
Accessing Recipes from "Mid-Fire Glazes" book in Insight-Live
Adjusting the Thixotropy of an Engobe for Pottery
Analysing a Crazing, Cutlery-marking Glaze Using Insight-Live
Compare the Chemistry of Recipes Using Insight-Live
Connecting an External Image to Insight-Live Pictures
Converting G1214M Cone 6 transparent glaze to G1214Z matte
Create a Synthetic Feldspar in Insight-Live
Creating a Cone 6 Oil-Spot Overglaze Effect
Design a Triangular Pottery Plate Block Mold in Fusion 360
Designing a Jigger Mold for a Bowl Using Fusion 360 CAD
Downloading and 3D-Printing a 3MF file
Draw a propeller in Fusion 360 for use on an overhead propeller mixer
Drawing a Mug Handle Mold in Fusion 360
Drawing a Mug Mold Using OnShape CAD
Enter a Recipe Into Insight-live
Entering TestData Into Insight-Live
Fine tune the thixotropy of a glaze or engobe slurry
Getting Frustrated With a 55% Gerstley Borate Glaze
How I Developed the G2926B Cone 6 Transparent Base Glaze
How I Formulated G2934 Cone 6 Silky MgO Matte Glaze Using Insight-Live
How to Apply a White Slip to Terra Cotta Ware
How to Paste a Recipe Into Insight-live
Importing Data into Insight-live
Importing Desktop Insight Recipes to Insight-live
Importing Generic CSV Recipe Data into Insight-Live
Insight-Live Meets a Silica Deprived Glaze Recipe
Insight-Live Quick Tour
Liner Glazing a Stoneware Mug
Make a precision plaster mold for slip casting using Fusion 360 and 3D Printing
Making ceramic glaze flow test balls
Making test bars for the SHAB, LDW and DFAC tests
Manually program your kiln or suffer glaze defects!
Mica and Feldspar Mine of MGK Minerals
Predicting Glaze Durability by Chemistry in Insight-Live
Preparing Pictures for Insight-live
Replace Lithium Carbonate With Lithium Frit Using Insight-Live
Replacing 10% Gerstley Borate in a clear glaze
Same Beer Bottle Mold Using Fusion 360 and OnShape CAD
Signing Up at Insight-live.com
Signing-In at Insight-live.com
Slip cast a stoneware beer bottle
Substitute Ferro Frit 3134 For Another Frit
Substituting Custer Feldspar for Another in a Cone 10R Glaze Recipe
Thixotropy and How to Gel a Ceramic Glaze
Use Insight-live to substitute materials in a recipe
Watch Thixotropy Happen With a 20kg Batch of Dipping Glaze

How I Formulated G2934 Cone 6 Silky MgO Matte Glaze Using Insight-Live

I will show you how found a recipe on Facebook, assessed it, substituted my own materials, tested it, adjusted it.


Click here to watch this at youtube.com or click here to go to our Youtube channel

Transcript/Notes

Silky Mattes are more difficult at cone 6 than at cone 10. It is common to find ones that either gloss on slight over-firing, are too matte, are not durable (they cutlery mark), ones that have a poor functional surfaces (and stain easily) and ones that craze.

I found this recipe on Facebook, it was called "Moores Matte".. Let's take a look at it in Insight-live.

Gerstley borate 9

more.. Silica 30
Dolomite 17.5
EPK 20
Nepheline syenite 33.5
Whiting 2.5

Copy it, paste into Insight-live account, # as G2928

#1: Mattes need high Al2O3
-many recipes source most of it from feldspar, that brings in too much KNaO and crazing happens
-other recipes source it from alot of clay, the glaze shrinks and cracks during drying

Open G2571A beside.

-Silky mattes happen when Al2O3 and MgO are high, SiO2 is low and the glaze melts well. Tiny surface ripples happen.
-At cone 10 it just happens. But at cone 6 it needs an extra kick with B2O3
-G2571A even has a little B2O3 (unusual but maybe a secret to why it works so well).
-At cone 6 we need more

Where do we get B2O3: GB (click it)
-This is going to have plenty of clay, we don't need GB gelling the slurry and shrinking it more (it is plastic)
Use a frit.

Open Roy Limits cone 6.
Compare limits again:
-MgO still not too high, Al2O3, SiO2 good, ratio is good

Sourcing issues again:
-The MgO is sourcing from dolomite: No good for cone 6, will use talc, melts better, no gasing
-CaO from whiting: switch to wollastonite to avoid gassing issues
-Clay: Not looking for toilet bowl white. Going to use Ravenscrag Slip to get a slurry of the best possible application properties (as much as I can)

Let's improve this recipe.
Not going to duplicate, going to start from scratch

1. Start with 50 Ravenscrag, 10 Frit
-click on RSlip to show iron

2. Add 1 talc, show it, match MgO (to 5)

3. Highlight B2O3, reduce frit to match it (to 6)

4. Highlight KNaO, need it, add 5 nepheline syenite, show it, re-hilight KNaO, match (to 7)

5. Increase frit to rematch boron (to 7)

6. Add 1 wollastonite, show it (oversupplies CaO, will leave for a moment)

7. Need Al2O3, SiO2. Add 1 silica, calcined kaolin

8. Add nepsy to 0.24, backoff (to 9)

9. Add 1 talc (to 6) to match MgO

9. Add frit (to 8) to rematch B2O3

10. Hi-light Al2O3, kaolin to 3.5

11. SiO2 to 1.5

Look at the LOI! It is much lower on this new glaze, that means less change of glaze defects.

Retotal to 100
Reduce RSlip to 60, notice formula hardly changes. Why? RSlip chemistry is much more like a glaze than any of the others.

It tested it. Too glossy. Needed to add Al2O3, increased Al2O3 to 0.5+

Calcined kaolin a good way to adjust: why? Try it.
-Cuts Al2O3 and SiO2 (increasing flux) and also increases the ratio a little.

Approximate final recipe:
Nepheline syenite 13
Ravenscrag Slip 60
Ferro Frit 3134 11
Talc 8
Wollastonite 1.5
Calcined Kaolin 9
Tin Oxide 5

Where is this going?
-Double layering
-Black matte

Mattes are fragile, glazes want to be glossy.
-It is important to have a way to adjust the degree of gloss so you can crank up the matte, then back off if it marks or stains
Frit 3134 only version also possible: show
Frit 3134/talc version: show



Links

Recipes G2928C - Ravenscrag Silky Matte for Cone 6
Plainsman Cone 6 Ravenscrag Slip based glaze. It can be found among others at http://ravenscrag.com.
URLs https://digitalfire.com/university/insight-live/overview/Insight-Live%20Overview.html
Insight-Live.com Overview Video
URLs http://m.youtube.com/user/tonywilliamhansen
YouTube channel for Tony Hansen
Glossary Matte Glaze
Random material mixes that melt well overwhelmingly want to be glossy, creating a matte glaze that is also functional is not an easy task.
Glossary Glaze Chemistry
Glaze chemistry is the study of how the oxide chemistry of glazes relate to the way they fire. It accounts for color, surface, hardness, texture, melting temperature, thermal expansion, etc.

Click here for case-studies of Insight-Live fixing problems


Insight-live help button

This picture has its own page with more detail, click here to see it.

You will see examples of replacing unavailable materials (especially frits), fixing various issues (e.g. running, crazing, settling), making them melt more, adjusting matteness, etc. Insight-Live has an extensive help system (the round blue icon on the left) that also deals with fixing real-world problems and understanding glazes and clay bodies.