2019 Jiggering-Casting Project of Medalta 66 Mug
A cereal bowl jigger mold made using 3D printing
Beer Bottle Master Mold via 3D Printing
Better porosity for Brown Sugar Savers
Build a kiln monitoring device
Celebration Project
Coffee Mug Slip Casting Mold via 3D Printing
Comparing the Melt Fluidity of 16 Frits
Cookie Cutting clay with 3D printed cutters
Evaluating a clay's suitability for use in pottery
Make a mold for 4-gallon stackable calciners
Make Your Own Pyrometric Cones
Make your own sieve shaker to process ceramic slurries
Making a high quality ceramic tile
Making a Plaster Table
Making Bricks
Making our own kiln posts using a hand extruder
Medalta Ball Pitcher Slip Casting Mold via 3D Printing
Medalta Jug Master Mold Development
Mold Natches
Mother Nature's Porcelain - Plainsman 3B
Mug Handle Casting
Nursery plant pot mold via 3D printing
Pie-Crust Mug-Making Method
Plainsman 3D, Mother Nature's Porcelain/Stoneware
Pottery Classes
Project to Document a Shimpo Jiggering Attachment
Roll, Cut, Pull, Attach Handle-making Method
Seven reasons to do DIY underglazes
Slurry Mixing and Dewatering Your Own Clay Body
Testing a New Load of EP Kaolin
Using milk as a glaze
Videos of factory workers making holloware
Yixing Teapots

Nursery plant pot mold via 3D printing

This was about producing the simplest of shapes, open and flared-out. But it was also about achieving a fairly precise fired size so that a standard plastic nursery pot would drop down inside in such a way that, after the plant had reached a specific size, it would be easy to grab it by the rim and extract it. Another aspect of this process was the idea of repeatedly printing a shell mold, pouring a working mold, casting a piece, firing it and trying the plastic pot.

I used my standard jigger shell mold. That enables dropping the freshly-cast pieces in and finishing the lips on my wheel.

Related Information

Nursery Plant Pot drawing


This picture has its own page with more detail, click here to see it.

I made the bottom and top radiuses and the height parametric. I made the diameter of the pouring ring = top diameter of the pot + 2 mm. The walls are 2mm thick because my 3D printer prints 0.4mm wide (that means two passes for each layer).

Easier way to make a plant pot mold via 3D printing


This picture has its own page with more detail, click here to see it.

Top left: I have 3D printed a shell mold, and filled it will plaster to produce the model.
Bottom left: I stuck it down to a smooth Arborite the batt using a sticky clay slip and have smoothed the model on the wheel (using a metal rib and sandpaper). Then I soaped it.
Bottom center: Glue the jigger head shell mold down using the same clay slip.
Bottom right: Fill that with plaster.
Top right: The mold is ready.
Top center: I attached a pouring spout and filled the mold with a red stoneware slip to produce this piece.
Top center: Notice how the plastic nursery pot fits: Its rim is still too far down to be able to grasp and remove it easily (and the top diameter of the clay pot is a little too much). 3D printing makes adjusting the the size easy.

Plant pot casting mold and my aluminum jigger head


This picture has its own page with more detail, click here to see it.

These molds do not need to fit into my jigger wheel, but it is handy if they do because I can do finishing on them before extracting the piece.

Using clay as a glue to hold a 3D-printed jigger mold in place


This picture has its own page with more detail, click here to see it.

This was part of my nursery plant-pot mold-making project. I held previous shell-molds down with a brick on top. But that was not working well, putting the mold out of shape, making it difficult to pour the slip inside and agitate the mold after pouring to surface the bubbles. I found that the 3D printed mold can be held down by simply using a sticky clay slip (Plainsman Polar Ice)! I printed this one with a flange at the bottom for this purpose. I am pouring the mold on an arborite bat on the wheelhead of a potters wheel. This enables turning the wheel slowly and pouring the plaster into the perimeter slowly through a funnel, that produces a much better surface. If you don't have a super sticky clay you can make one by adding 4% Veegum to a Grolleg porcelain. Actually, Grolleg and New Zealand kaolins are both very sticky, so they could also work.

My potter's wheel with aluminum cup-head and jigger mold inserted


This picture has its own page with more detail, click here to see it.

The cup-head was lathed from a block of aluminum and it attaches to the shaft the same as a regular wheel-head. Plaster molds simply drop in and sit on their shoulder. The shoulder is the only point-of-contact, this prevents chattering while the mold spins when under pressure. I am using these molds for a casting-jiggering process (or just casting). For example, I can cast a mug in the mold, then pour out the slip, wait a few minutes and then, as the wheel spins, finish the rim and inside sure using a 3D-printed template/rib. I do not actually use the jigger arm, it is easier just to hold the template in hand. I can finish the rims on any round pieces made in these molds.

Links

Projects Beer Bottle Master Mold via 3D Printing
A project that took several years of failures and blind allies and is finally coming together - so much simpler than expected!
Projects A cereal bowl jigger mold made using 3D printing
A new way to 3D-print your way to making jigger molds and templates. The molds are encased in a 3D printed shell that makes them fit perfectly into the cuphead. And the template is precise and very effectivwe.
Projects Medalta Ball Pitcher Slip Casting Mold via 3D Printing
A project to make a reproduction of a Medalta Potteries piece that was done during the 1940s. This is the smallest of the three sizes they made.
Projects Coffee Mug Slip Casting Mold via 3D Printing
A potter can now use AI, 3D CAD, 3D printing and custom clay bodies to slip-cast beautiful quality stoneware pottery mugs. It is efficient and practical.
Typecodes Mold making using 3D printing
An ordinary consumer 3D printer has many exciting possibilities for making many types of molds, it is a place where people having both artistic and mechanical abilities can get a double the dopamine!

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 