Oct 22, 2026: We are working on protecting our servers against the PHP2Shell vulnerability recently discovered. Servers were upgraded ahead of schedule on Oct 21. This could cause some issues. Please contact us if you encounter any.

1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Stains Mason

Description: MASON STAINS

Notes

Color sample tiles for Mason stains are produced using stain/opacifier mixes as follows:

If stain is 10% opacifier is 10%, 6% - 2%, 5% - 10%, 2% - 5%

Pinks contain 10% stain and 1.5% zirconium opacifier.

All samples are mixed with a zincless glaze composed of 85% cone 01-1 leadless frit and 15% clay.

Related Information

Mason stains in G2916F cone 6 clear base


This picture has its own page with more detail, click here to see it.

These are Mason stains added to cone 6 G2916F clear liner base glaze. Notice that all of these stains develop the correct colors with this base (except for manganese alumina pink 6020). However caution is required with inclusion stains (like #6021), if they are rated to cone 8 they may already begin bubbling at cone 6 is some host glazes.

Mason stains in the G2926B base glaze at cone 6


19 glazed porcelain tiles showcasing Mason stain colors

This picture has its own page with more detail, click here to see it.

This glaze, G2926B, is our main glossy base recipe. Stains are a much better choice for coloring it than raw metal oxides. Other than the great colors they produce here, there are a number of things worth noticing.
-Stains are potent; the percentages needed are normally much less than for metal oxides.
-Staining a transparent glaze produces a transparent color, it is more intense where the laydown is thicker - this is often desirable in highlighting contours and designs. For pastel shades, add an opacifier (e.g. 5-10% Zircopax, more stain might be needed to maintain the color intensity).
-The chrome-tin maroon 6006 does not develop well in this base (alternatives are G2916F or G1214M).
-The 6020 manganese alumina pink is also not developing here (it is a body stain).
-Caution is required with inclusion stains (like #6021). Bubbling, as is happening here, is common - this can be mitigated by adding 1-2% Zircopax.
-And it’s easy to turn any of these into brushing glazes or dipping glazes. Be sure to blender mix them to break up any agglomerates.

Mason stains in the G2934 matte base glaze at cone 6


Glazed porcelain tiles

This picture has its own page with more detail, click here to see it.

Stains can work surprisingly well in matte base glazes like the DIY G2934 recipe. The glass is less transparent and so varying thicknesses do not produce as much variation in tint as glossy bases do. Notice how low many of the stain percentages are here, yet most of the colors are bright. We tested 6600, 6350, 6300, 6021 and 6404 overnight in lemon juice, they all passed leach-free. The 6385 is an error, it should be purple (that being said, do not use it, it is ugly in this base). And chrome-tin pink and maroon stains do not develop the color (e.g. 6006). But our G1214Z1 CaO-matte comes to the rescue, it both works better with some stains and has a more crystal matte surface. The degree-of-matteness of both can be tuned by cooling speed and blending in some G2926B glossy base. You can mix any of these into a brushing glaze or a dipping glaze. Be sure to blender mix them to break up any agglomerates.

How to include stains in chemistry calculations in Insight


This picture has its own page with more detail, click here to see it.

The simple answer is that you should not. The chemistry of stains is proprietary. Stain particles do not dissolve into the glaze melt like other materials, they suspend in the transparent glass to color it. That is why stains are color stable and dependable. In addition, their percentage in the recipe, not the formula, is the predictor of their effect on the fired glaze. Of course they do impose effects on the thermal expansion, melt fluidity, etc., but these must be rationalized by experience and testing. But you can still enter stains into Insight recipes. Consider adding the stains you use to your private materials database (for costing purposes for example).

Links

Oxide Analysis Formula Tolerance
Materials Stain
Typecodes Colorant
Metallic based materials that impart fired color to glazes and bodies.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy