1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

McNamee Kaolin

Description: South Carolina Kaolin

Oxide Analysis Formula Tolerance
CaO 0.06% -
K2O 0.30% 0.01
MgO 0.05% -
Na2O 0.05% -
TiO2 1.20% 0.04
Al2O3 39.30% 1.00
SiO2 44.50% 1.92
Fe2O3 0.33% 0.01
LOI 14.00%n/a
Oxide Weight 222.66
Formula Weight 258.91

Notes

A plastic kaolin from South Carolina (Bath Township, Aiken County) by the Dixie Clay company (owned by R. T. Vanderbilt). It is open-pit-mined, dry-milled, air-classified and sold under different trade names (depending on the particle size). McNamee kaolin is the largest of the sizes and they refer to it as the "softest" (th e powder is fluffy). It has similar properties to Pioneer Kaolin. The leather hard material feels soapy on cut edges.

It is mainly targeted at the rubber industry, but in ceramics its is often used for white stoneware bodies. Noted for peach blush that occurs when fired in gas kilns. It is also suitable in porcelain bodies.

Related Information

McNamee kaolin (left) vs. Pioneer Kaolin (right) at cone 6


This picture has its own page with more detail, click here to see it.

Both of these are a kaolin:nepheline syenite blend (mixed 70:30, which produces a zero-porosity (zero measured water absorption) body around cone 9 for an American kaolin). Both of these have about 2.5% porosity at cone 6, they respond similarly to the glaze, and the fired color is very similar. The McNamee clay has a 1% higher fired shrinkage (10.5% vs. 9.5%), and it requires a little more water to get the same plasticity.

Links

Materials PAR Kaolin
Materials Dixie Clay
Materials Peerless 2 Kaolin
Materials Langford Kaolin
Materials Bilt-Cote Kaolin
Materials Peerless 3 Kaolin
Materials Kaolin
The purest of all clays in nature. Kaolins are used in porcelains and stonewares to impart whiteness, in glazes to supply Al2O3 and to suspend slurries.
Materials Pioneer Kaolin
Typecodes Kaolin
Pure clay mineral, there are many brand names of varying purity and iron content.

Data

GE Brightness 75
% Passing 325 Mesh Wet 99.65%
Moisture Content - Powder 1% Max
pH for dry powder 4.8

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy