Description: Kentucky Ball Clay
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.12% | 0.01 | |
| K2O | 0.83% | 0.04 | |
| MgO | 0.27% | 0.03 | |
| Na2O | 0.05% | - | |
| TiO2 | 1.88% | 0.09 | |
| Al2O3 | 25.45% | 1.00 | |
| SiO2 | 60.00% | 4.00 | |
| Fe2O3 | 1.06% | 0.03 | |
| LOI | 9.80% | n/a | |
| Oxide Weight | 359.34 | ||
| Formula Weight | 398.39 | ||
Crude Color: Tan
Dry M.O.R. (psi 50% clay/50% flint, cast bars): 475
Wet Sieve Residue, +200 mesh (%): 0.45
Water of Plasticity (%): 33
Linear Dry Shrinkage (%): 6.7
Solubles Sulfates (ppm): 350
Filtration (ml): 23
Specific Surface Area (sq meters per gram): 19.4
CEC/MBI (meq/100 ml): 9.5
pH: 6.3
PCE: 31
Firing Shrinkage (%)
Cone 04: 4.0
Cone 3: 6.3
Cone 11: 7.1
Absorption (%)
Cone 04: 14.2
Cone 3: 7.5
Cone 11: 3.0
Particle Size (% finer than):
50 microns: 100
20: 97
10: 91
5: 82
1: 59
0.5: 48
| Materials |
5-S Ball Clay
|
| Materials |
Ball Clay
A fine particled highly plastic secondary clay used mainly to impart plasticity to clay and porcelain bodies and to suspend glaze, slips and engobe slurries. |
| Typecodes |
Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites. |
| Dry M.O.R. (50% Silica) | 1537C |
|---|