Description: Kentucky Ball Clay
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.04% | - | |
| K2O | 0.80% | 0.03 | |
| MgO | 0.18% | 0.02 | |
| Na2O | 0.12% | 0.01 | |
| TiO2 | 1.58% | 0.07 | |
| Al2O3 | 28.60% | 1.00 | |
| SiO2 | 57.40% | 3.41 | |
| Fe2O3 | 0.98% | 0.02 | |
| LOI | 9.60% | n/a | |
| Oxide Weight | 319.91 | ||
| Formula Weight | 353.88 | ||
Crude Color: White
Dry M.O.R. (psi 50% clay/50% flint, cast bars): 300
Wet Sieve Residue, +200 mesh (%): 0.64
Water of Plasticity (%): 32
Linear Dry Shrinkage (%): 6.0
Solubles Sulfates (ppm): 200
Filtration (ml): 25
Specific Surface Area (sq meters per gram): 18.9
CEC/MBI (meq/100 ml): 9.0
pH: 5.8
PCE: 30
Firing Shrinkage (%)
Cone 04: 5.3
Cone 3: 7.2
Cone 11: 8.0
Absorption (%)
Cone 04: 13.5
Cone 3: 9.8
Cone 11: 3.6
Particle Size (% finer than):
50 microns: 100
20: 96
10: 94
5: 87
1: 62
0.5: 51
| Materials |
54-S Ball Clay
|
| Materials |
Ball Clay
A fine particled highly plastic secondary clay used mainly to impart plasticity to clay and porcelain bodies and to suspend glaze, slips and engobe slurries. |
| Typecodes |
Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites. |
| Dry M.O.R. (50% Silica) | 774C |
|---|