Description: Tennessee Ball Clay
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.05% | - | |
| K2O | 0.47% | 0.02 | |
| MgO | 0.18% | 0.02 | |
| Na2O | 0.08% | - | |
| TiO2 | 1.70% | 0.08 | |
| Al2O3 | 26.90% | 1.00 | |
| SiO2 | 59.90% | 3.78 | |
| Fe2O3 | 1.08% | 0.03 | |
| LOI | 9.60% | n/a | |
| Oxide Weight | 342.63 | ||
| Formula Weight | 379.01 | ||
Crude Color: Grey
Dry M.O.R. (psi 50% clay/50% flint, cast bars): 420
Wet Sieve Residue, +200 mesh (%): 0.38
Water of Plasticity (%): 38
Linear Dry Shrinkage (%): 8.0
Solubles Sulfates (ppm): 196
Filtration (ml): 24
Specific Surface Area (sq meters per gram): 21.3
CEC/MBI (meq/100 ml): 11.0
pH: 5.0
PCE: 31-32
Firing Shrinkage (%)
Cone 04: 6.6
Cone 3: 7.3
Cone 11: 8.3
Absorption (%)
Cone 04: 17.9
Cone 3: 11.7
Cone 11: 4.2
Particle Size (% finer than):
50 microns: 100
20: 97
10: 90
5: 82
1: 63
0.5: 51
| Materials |
Ball Clay
A fine particled highly plastic secondary clay used mainly to impart plasticity to clay and porcelain bodies and to suspend glaze, slips and engobe slurries. |
| Typecodes |
Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites. |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk