Thomas Ball Clay

Description: Tennessee Ball Clay

Oxide Analysis Formula Tolerance
CaO 0.06% -
K2O 0.40% 0.02
MgO 0.20% 0.02
Na2O 0.08% -
TiO2 1.60% 0.08
Al2O3 26.50% 1.00
SiO2 59.40% 3.80
Fe2O3 1.02% 0.02
LOI 10.60%n/a
Oxide Weight 343.57
Formula Weight 384.30

Notes

Crude Color: Brown
Dry M.O.R. (psi 50% clay/50% flint, cast bars): 511
Wet Sieve Residue, +200 mesh (%): 0.31
Water of Plasticity (%): 36
Linear Dry Shrinkage (%): 7.26
Solubles Sulfates (ppm): 283
Filtration (ml): 26
Specific Surface Area (sq meters per gram): 19.8
CEC/MBI (meq/100 ml): 10.5
pH: 5.3
PCE: 31

Firing Shrinkage (%) Cone 04: 5.9 Cone 3: 7.0 Cone 11: 8.0
Absorption (%) 16.2 10.8 4.0

Particle Size (% finer than):
50 microns: 100
20: 96
10: 93
5: 85
1: 65
0.5: 54

Related Information

Links

Materials Cooley No. 2 Ball Clay
Materials Ball Clay
A fine particled highly plastic secondary clay used mainly to impart plasticity to clay and porcelain bodies and to suspend glaze, slips and engobe slurries.
Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy