Description: Tennessee Ball Clay
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.03% | - | |
| K2O | 0.50% | 0.02 | |
| MgO | 0.21% | 0.02 | |
| Na2O | 0.08% | - | |
| TiO2 | 1.50% | 0.07 | |
| Al2O3 | 27.40% | 1.00 | |
| SiO2 | 59.30% | 3.67 | |
| Fe2O3 | 1.10% | 0.03 | |
| LOI | 9.28% | n/a | |
| Oxide Weight | 335.48 | ||
| Formula Weight | 369.80 | ||
Crude Color: Light Grey
Dry M.O.R. (psi 50% clay/50% flint, cast bars): 521
Wet Sieve Residue, +200 mesh (%): 0.21
Water of Plasticity (%): 39
Linear Dry Shrinkage (%): 7.43
Solubles Sulfates (ppm): 235
Filtration (ml): 24
Specific Surface Area (sq meters per gram): 20.2
CEC/MBI (meq/100 ml): 11.0
pH: 5.3
PCE: 31
Firing Shrinkage (%) Cone 04: 6.4 Cone 3: 7.5 Cone 11: 8.7
Absorption (%) 16.1 10.2 3.8
Particle Size (% finer than):
50 microns: 100
20: 97
10: 91
5: 80
1: 60
0.5: 52
| Materials |
Ball Clay
A fine particled highly plastic secondary clay used mainly to impart plasticity to clay and porcelain bodies and to suspend glaze, slips and engobe slurries. |
| Typecodes |
Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites. |