Bell Dark Ball Clay

Description: Tennessee Ball Clay

Oxide Analysis Formula Tolerance
CaO 0.20% 0.01
K2O 0.70% 0.03
MgO 0.40% 0.04
Na2O 0.20% 0.01
TiO2 2.10% 0.10
Al2O3 26.80% 1.00
SiO2 58.90% 3.73
Fe2O3 1.10% 0.03
LOI 10.30%n/a
Oxide Weight 344.06
Formula Weight 383.57

Notes

A very plastic ball clay used in industrial and hobby clay bodies of all types. Primary applications are dinnerware and artware.

Physical Properties
===================
Water of Plasticity: 33.5%
% Dry Shrinkage: 6.1
Dry M.O.R. (50:50 ball clay:silica) psi:* 560
pH: 4.1
M.B.I. meq/100g: 8.0
Specific Surface Area (sq-metre/g): 24.1
Soluble sulfur+: Low

P.C.E.: 38

Particle Size, Microns: 20 10 5 2 1 0.5 0.2
(% finer than) 99% 94% 85% 75% 63% 52% 38%

Fired Properties
================
Cone 5 10
----
Total Shrinkage: 12.7% 15.6%
Absorption: 12.5% 6.1%

------------------
*Extruded, 50% ball clay, 50% flint
+Low-trace to 150, Med-150-400, High-450+
**50% Clay, 50% Nepheline Syenite

*This information is from a data sheet dated Jan 2013.

Related Information

Links

Materials Ball Clay
A fine particled highly plastic secondary clay used mainly to impart plasticity to clay and porcelain bodies and to suspend glaze, slips and engobe slurries.
Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

Data

Dry M.O.R. (50% Silica) 1482C

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy