| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 1.81% | 0.24 | |
| MgO | 0.14% | 0.03 | |
| K2O | 4.31% | 0.34 | |
| Na2O | 3.30% | 0.40 | |
| Fe2O3 | 0.20% | 0.01 | |
| TiO2 | 0.15% | 0.01 | |
| Al2O3 | 16.33% | 1.19 | |
| SiO2 | 73.76% | 9.11 | |
| Oxide Weight | 742.30 | ||
| Formula Weight | 742.30 | ||
In order to create a substitute, I had to come up with an average analysis (because this was a variable material).
| CORNWALL STONE Average Calculation | ||||||||||
| MATERIAL | PARTS | WEIGHT | *CaO | *MgO | *K2O | *Na2O | *Fe2O3 | *TiO2 | Al2O3 | SiO2 |
| Oxide Weights | 56.1 | 40.3 | 94.2 | 62.0 | 160.0 | 79.7 | 102.0 | 60.0 | ||
| NUMBER 1 | 500.00 | 640.93 | .16 | .05 | .22 | .33 | .01 | .01 | .76 | 6.02 |
| NUMBER 2 | 500.00 | 682.90 | .17 | .03 | .25 | .27 | .01 | .01 | .74 | 6.06 |
| NUMBER 3 | 500.00 | 680.57 | .22 | .01 | .20 | .29 | .00 | .01 | .78 | 6.02 |
| NUMBER 4 | 500.00 | 705.21 | .19 | .01 | .23 | .26 | .01 | .01 | .78 | 6.00 |
| NUMBER 5 | 500.00 | 717.95 | .15 | .03 | .22 | .28 | .01 | .01 | .76 | 6.08 |
| NUMBER 6 | 500.00 | 696.23 | .16 | .01 | .11 | .42 | .00 | .01 | .79 | 6.07 |
| NUMBER 7 | 500.00 | 718.73 | .19 | .02 | .22 | .25 | .01 | .01 | .79 | 6.02 |
| NUMBER 8 | 500.00 | 736.85 | .19 | .03 | .21 | .24 | .01 | .01 | .76 | 6.09 |
| NUMBER 9 | 500.00 | 1118.35 | .08 | - | .25 | .10 | .01 | .01 | .83 | 6.12 |
| NUMBER 10 | 500.00 | 963.42 | .08 | - | .20 | .22 | .01 | .01 | .83 | 6.07 |
| NUMBER 11 | 500.00 | 685.63 | .19 | .01 | .35 | .18 | .00 | - | .82 | 5.90 |
| NUMBER 12 | 500.00 | 738.13 | .12 | .01 | .24 | .29 | .01 | .00 | .78 | 5.97 |
| TOTAL | 6000.00 | 1.90 | .21 | 2.70 | 3.13 | .07 | .11 | 9.43 | 72.42 | |
| UNITY FORMULA | .23 | .03 | .33 | .39 | .01 | .01 | 1.16 | 8.92 | ||
| Average Precentage Analysis | 1.81 | .14 | 4.31 | 3.30 | .20 | .15 | 16.33 | 73.76 | ||
This became the target for our L3617 Cornwall Stone substitute recipe.
There are two ways to use this: Weigh up a batch, mix it thoroughly, then treat it as a raw material (if you are confident enough in being able to shake the mix enough to mix it really well). Otherwise, re-total the recipe for the Cornwall substitute to the amount needed in your recipe and then combine the two recipes. Actually, both of these approaches have a small issue. The L3617 recipe contains materials that have an LOI, its total calculated LOI is 2.4%. That means the most correct amount to substitute for 20.3 is 20.3/(100-0.27/100) or 20.8.

This picture has its own page with more detail, click here to see it.
This is a cone 11 oxidation melt flow test. Shown (left to right):
-A new shipment of Cornwall Stone 2011
-L3617 Digitalfire calculated substitute recipe
-An older Cornwall shipment
-The H&G substitute 2011 (far right, mislabelled on the picture).
These do not flow well here, a small frit addition was later employed to better compare them. However they have melted enough to see some differences in whiteness and degree of melt. Notice the L3617 is more like the old Cornwall Stone than the new Cornwall is.

This picture has its own page with more detail, click here to see it.
These melt flow GLFL tests compare my Cornwall Stone substitute recipe with the original material (no longer available in North America). 20% Frit 3134 was added to each to enable sufficient melting at cone 5 (the melts do not flow even at cone 11 without the frit). L3617A is Cornwall Stone (plus the frit), and L3619A is the substitute (plus the frit).
This substitute, L3617, is chemically equivalent to an average of many analyses of Cornwall Stone (which varied significantly). The substitute recipe has a distinct advantage: It contains common ceramic materials (G-200 EU Feldspar, Nepheline Syenite, Dolomite,
Wollastonite, Pioneer Kaolin, Silica) and has the potential to be much more consistent than the original material was.
| Materials |
Cornwall Stone
Cornwall stone was a low-iron feldspar material used primarily as a flux in clay bodies and glazes |
| Articles |
Substituting Cornwall Stone
Calculating a recipe of materials having the same oxide chemistry as Cornwall Stone |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk