Tennessee #6 Bond

Description: Tennessee Ball Clay

Oxide Analysis Formula Tolerance
CaO 0.30% 0.02
K2O 1.40% 0.06
MgO 0.05% -
Na2O 0.20% 0.01
TiO2 2.00% 0.09
Al2O3 27.20% 1.00
SiO2 59.40% 3.71
Fe2O3 0.80% 0.02
LOI 9.50%n/a
Oxide Weight 342.56
Formula Weight 378.52

Notes

An intermediate-grained Ball Clay with good plasticity and strength. Tennessee #6 Bond is primarily used in refractory applications. It is also very popular in wet sodium silicate mortars based on its excellent shelf life and trowelability.

Physical Properties
===================
Water of Plasticity*: 37.0%
% Dry Shrinkage*: 6.5
Dry M.O.R., psi:* 825
pH: 4.4
C.E.C., meq/100g: 11.0
Specific Surface Area, sq metre/g: 24.4
Soluble sulfur+: Low

P.C.E.: 32

Particle Size, Microns: 20 10 5 2 1 0.5 0.2
(% finer than) 99% 97% 93% 81% 72% 56% 35%

Fired Properties
================
Cone 5 10
----
Total Shrinkage: 13.0% 14.5%
Absorption: 10.0% 1.0%

------------------
*Extruded, 50% ball clay, 50% flint
+Low-trace to 150, Med-150-400, High-450+
**50% Clay, 50% Nepheline Syenite

Related Information

Links

Materials Ball Clay
A fine particled highly plastic secondary clay used mainly to impart plasticity to clay and porcelain bodies and to suspend glaze, slips and engobe slurries.
Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy