Alternate Names: Cyprus Glacier 200 Talc
Description: Montana Talc
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 2.00% | 0.05 | |
| MgO | 30.00% | 0.95 | |
| Al2O3 | 0.50% | 0.01 | |
| SiO2 | 60.00% | 1.28 | |
| Fe2O3 | 1.00% | 0.01 | |
| CO2 | 2.50% | n/a | |
| H2O | 4.00% | n/a | |
| Oxide Weight | 119.86 | ||
| Formula Weight | 128.19 | ||
Glacier 200 platy talc is the filler or extender of choice in dark-colored paints and primers, and for many other applications without high brightness requirements. Cyprus offers Glacier 200 at a substantial cost savings compared with higher brightness talcs.
Mineral Analysis:
Talc: 94%
Dolomite: 2%
Calcite: 2%
Quartz: 2%
Asbestos Minerals: not detected
Oil Absorption, g/100g talc:
Spatula rub-out, ASTM D281 - 28
Gardner-Coleman, ASTM D1483 - 38
Apparent Density, lb/ft3:
Loose (Scott Volumeter) - 28
Tapped (Numinco) - 61
Surface Area, m2/g (N2, BET) - 9
Hegman Fineness of Grind: 1.5-2.5
Adsorbed Moisture, %: .2
pH (1:5 dilution): 9
Refractive Index: 1.6
Specific Gravity: 2.8
Particle Size:
Minus 200 mesh, 74 micron: 99.6-99.8%
-325 mesh, 44 micron: 96%
-20 micron: 84%
-10 micron: 57%
-5 micron: 36%
-2 micron: 18%
-1 micron: 10%
Median Particle Size, micron: 8
| Materials |
Talc
A source of MgO for ceramic glazes, a flux or thermal expansion additive in clay bodies, also used in the manufacture of cordierite. |
| Typecodes |
Flux Source
Materials that source Na2O, K2O, Li2O, CaO, MgO and other fluxes but are not feldspars or frits. Remember that materials can be flux sources but also perform many other roles. For example, talc is a flux in high temperature glazes, but a matting agent in low temperatures ones. It can also be a flux, a filler and an expansion increaser in bodies. |
| Hazards |
Talc Hazards Overview
Talc is invaluable in the ceramics industry, it is used as a glaze and body ingredient and as a parting a release agent in various processes. Is it safe? |