Oct 22, 2026: We are working on protecting our servers against the PHP2Shell vulnerability just discovered. The CDN download server is back online. The digitalfire and insight-live servers were patched on Oct 21.
Alternate Names: Lithium Mica
Formula: LiF.KF.Al2O3.3SiO2
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| K2O | 7.30% | 0.43 | |
| Li2O | 3.00% | 0.57 | |
| Al2O3 | 26.90% | 1.48 | |
| SiO2 | 47.70% | 4.45 | |
| H2O | 4.70% | n/a | |
| LOI | 10.00% | n/a | |
| Oxide Weight | 476.52 | ||
| Formula Weight | 558.64 | ||
It has a lower fusion point than most high temperature feldspars. The fluorine content can cause problems with glaze bubbles and surface pitting.
It is tricky to establish a formula weight and analysis for this material. Here are some of the factors:
-LOI varies, but we have assumed 5% water in this example.
-Lepidolite does not actually contain Li2O, it has to absorb oxygen from the atmosphere or other materials during firing since the Li is bonded to F.
-Fluorine is bonded to potassium so oxygen has to be absorbed to create K2O.
-For both Li and K only 1/2 of a molecule per input molecule of lepidolite will be yielded.
-In a complete oxidation firing all of the fluorine will volatilize and none will be in the final glass. However in real world conditions neither of these is likely to happen completely, and in a reduction firing neither may happen at all. In this case we are assuming it is all LOI.
Given the above assumptions, an input of LiF.KF.Al2O3.3SiO2 would yield:
1/2 Li2O
1/2 K2O
2 F
1 Al2O3
3 SiO2
5 LOI
Considering the F as LOI we would have the chemistry quoted here.
To properly handle a material like this in glaze chemistry fluorine conversion factors have to be employed.

This picture has its own page with more detail, click here to see it.

This picture has its own page with more detail, click here to see it.

This picture has its own page with more detail, click here to see it.
| URLs |
http://mineral.galleries.com/minerals/silicate/lepidoli/lepidoli.htm
Lepidolite at Mineral.galleries.com |
| URLs |
http://webmineral.com/data/Lepidolite.shtml
Lepidolite at WebMineral.com |
| URLs |
http://www.mindat.org/show.php?name=Lepidolite
Lepidolite at Mindat.org |
| URLs |
http://en.wikipedia.org/wiki/Lepidolite
Lepidolite at Wikipedia |
| Materials |
Lepidolite
|
| Materials |
Amblygonite
|
| Materials |
Petalite
|
| Materials |
Spodumene
Spodumene is a lithium sourcing feldspar, an alternative to lithium carbonate to supply Li2O to ceramic glazes. Contains up to about 8% Li2O. |
| Materials |
Triphylite
|
| Materials |
Mica
|
| Hazards |
Lithium Toxicology
|
| Typecodes |
Generic Material
Generic materials are those with no brand name. Normally they are theoretical, the chemistry portrays what a specimen would be if it had no contamination. Generic materials are helpful in educational situations where students need to study material theory (later they graduate to dealing with real world materials). They are also helpful where the chemistry of an actual material is not known. Often the accuracy of calculations is sufficient using generic materials. |
| Typecodes |
Feldspar
The most common source of fluxes for high and medium temperature glazes and bodies. |
| Oxides | Li2O - Lithium Oxide, Lithia |
| Minerals |
Lepidolite
Although this material is sometimes referred to as a lithium feldspar, it is not a feldspar, but rat |
| Density (Specific Gravity) | 3.00 |
|---|---|
| Frit Melting Range (C) | 1150-1300C |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk