Digitalfire is facing a takedown order from Plainsman Clays. They are revoking permission to "use any Plainsman content" "on any platform". This is broad and vague enough, and this site large enough, that I am unable to comply or even interpret it in the short timeframe (June 27). Please don't panic, I am overwhelmed by the unbelievable support I am getting. We just need to get them to relent on this demand and call off the lawyer (to at least permit commentary). There are lots of backup sites (many people have the API endpoints), don't start downloading or scraping again and overload the server.
Insight-live.com general operation is not affected by this.
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.01% | - | |
| K2O | 0.86% | 0.06 | |
| MgO | 0.09% | 0.01 | |
| Al2O3 | 16.30% | 1.00 | |
| SiO2 | 71.00% | 7.39 | |
| Fe2O3 | 0.53% | 0.02 | |
| TiO2 | 0.32% | 0.03 | |
| SO4 | 4.20% | n/a | |
| Oxide Weight | 557.62 | ||
| Formula Weight | 582.07 | ||
Sandy White is a naturally occurring blend of high quality silica (49%), Kaolin (42%), and feldspar(5%). It is used as a filler in clay bodies to increase both strength and workability.
The following shrinkage and porosity numbers from the supplier are implausible. The chemistry is also suspect since it only totals 93.
Sieve analysis: 0% on 80 mesh, 10% on 200 mesh
Drying shrinkage: 1.75%
Fired shrinkage: Cone 05 - 2%, cone 2%, cone 5 - 2%, cone 10 - 2%
Porosity: Cone 05 - 18.1%, cone 1 - 12.3%, cone 5 - 13.3%, cone 10 - 1.6%
| Typecodes |
Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically. |
| URLs |
https://www.clayimco.com/industrial-clays
IMCO information on their mined clays |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk