Tennessee #1 SGP

Alternate Names: SGP #1 Ball Clay

Description: Tennessee Ball Clay

Oxide Analysis Formula Tolerance
CaO 0.20% 0.01
K2O 0.60% 0.02
MgO 0.40% 0.04
Na2O 0.20% 0.01
TiO2 2.00% 0.10
Al2O3 26.80% 1.00
SiO2 58.90% 3.73
Fe2O3 1.10% 0.03
LOI 10.10%n/a
Oxide Weight 343.30
Formula Weight 381.87

Notes

A coarse-grained fast-casting ball clay with medium plasticity and strength. SGP is an "industry standard" based on its popularity in for casting. It can also be used in plastic formed bodies. It is also widely used as a suspension aid in glazes.

Physical Properties
===================
Water of Plasticity: 33.8%
% Dry Shrinkage: 6.2
Dry M.O.R. (50:50 ball clay:silica, psi): 580
pH: 4.5
M.B.I. (meq/100g): 8.7
Specific Surface Area (sq-meter/g): 24.7
Soluble sulphur SO4: Low

P.C.E.: 32

Particle Size, Microns: 20 10 5 2 1 0.5
(% finer than) 97% 94% 87% 76% 65% 54%

Fired Properties
================
Cone 5 10
Total Shrinkage: 13.0% 15.9%
Absorption: 12.5% 6.0%

Shipped from Mayfield, KY

*This info is from a data sheet from Jan 2013

Related Information

Links

Materials Ball Clay
A fine particled highly plastic secondary clay used mainly to impart plasticity to clay and porcelain bodies and to suspend glaze, slips and engobe slurries.
Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

Data

Pyrometric Cone Equivalent 32

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy