Description: Plainsman Native Clay

Oxide Analysis Formula Tolerance
BaO 0.32% 0.02
CaO 0.19% 0.03
K2O 2.57% 0.21
MgO 0.76% 0.14
Na2O 0.05% 0.01
TiO2 0.65% 0.06
Al2O3 13.54% 1.00
P2O5 0.55% 0.03
SiO2 72.26% 9.06
Fe2O3 4.10% 0.19
MnO 0.01% -
LOI 5.00%n/a
Oxide Weight 715.66
Formula Weight 753.32

Notes

A natural high iron, mid-temperature stoneware clay of good plasticity. It is particulary well suited to oxidation bodies in the middle temperature ranges. It is very deep red at cone 7-8.

Fired Temperature, Cone 4 5 6 7 8 9
--------------------------------------
Fired Shrinkage: 3.1% 3.4% 3.7% 4.0% 4.2% 4.4%
Absorption: 6.4% 5.0% 4.0% 3.5% 3.0% 1.9%
Fired Strength:
(lbs/ square inch) 5100 5300 5600 5900 6400

Sieve Analysis Wet Washed
(Root of 2 series) +35 +48 +65 +100 +150# +200 +325
--------------------------------------------
0.0% 0.3% 2.4% 5.1% 7.6% 10.0% 22.2%

Texture: Sl. tooth
Plastic Index (1-10): 5
Green Strength (lbs/sqaure inch): 850
Dry shrinkage: 5.0
Dried density: 2.05
PCE: 15.5

Related Information

Fire-Red and Restone fired test bars


This picture has its own page with more detail, click here to see it.

Plainsman Fire-Red (left) fired at cone 8,9,10,11 and 10R and Redstone (right) fired at cone 4,5,6,7,8.

Links

Materials M2 Red Stoneware
Materials Fire-Red
Materials Calvert Clay
Typecodes Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically.

Data

Pyrometric Cone Equivalent 15

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy